ABS (acrylonitrile butadiene styrene) is an amorphous thermoplastic in which a butadiene rubber phase provides toughness and the styrene-acrylonitrile matrix provides stiffness and a glossy, paintable surface. It is inexpensive and dimensionally stable, and it is easy to machine, mold, glue and paint, which is why it dominates consumer-electronics and appliance housings.
Choose ABS for indoor enclosures, covers, trim and prototype housings that must look and feel like production plastic, at the lowest cost among engineering plastics. Its limits are clear: it yellows and embrittles under UV, softens at roughly 80–100 °C, and is attacked by ketones, esters and many fuels. On Uretyco it is offered for CNC machining, injection molding and FDM printing.
Mechanical and physical properties
| Property | Typical value | Notes |
|---|---|---|
| Tensile strength (yield) | ≈ 40 MPa | ≈ 35–50 MPa across grades; FDM parts are lower, especially across layers. |
| Elongation at break | ≈ 10–50% | Strongly grade-dependent; high-impact grades at the top of the range. |
| Tensile modulus | ≈ 2.0–2.4 GPa | About 1/30 of aluminum; add stiffness with ribs rather than wall thickness. |
| Notched impact strength (Izod) | ≈ 150–400 J/m | ASTM D256, 23 °C. Tough for a low-cost plastic; PC is considerably tougher. |
| Density | ≈ 1.04–1.06 g/cm³ | One of the lightest engineering plastics. |
| Heat deflection temperature (HDT) | ≈ 80–100 °C | At 1.8 MPa; annealed parts at the upper end. |
| Max. continuous service temperature | ≈ 60–80 °C | Glass transition ≈ 105 °C; loaded parts creep and distort well before that. |
| Thermal expansion | ≈ 70–100 µm/m·K | 3–4× aluminum: a 200 mm part grows ≈ 0.14–0.2 mm per 10 °C. |
| Flammability | UL 94 HB | Standard grades burn; flame-retardant ABS grades reach V-0. |
| Machinability | Good | Cuts cleanly with sharp tools; softens at low temperature, so heat must be controlled. |
Typical room-temperature values for general-purpose injection-molding and extrusion grades of ABS. Properties vary considerably between grades (high-impact, high-heat, flame-retardant, plating grades) and between molded, machined and printed parts. For design calculations, use the data sheet of the specific grade named in your quote.
CNC machining ABS
ABS machines easily from sheet and rod with sharp carbide or HSS tools. Because it softens at low temperature, the main risks are heat and smeared edges rather than tool wear. Watch for:
- Heat: sharp tools and good chip evacuation (air or water-based coolant) prevent melting and gummy burrs; avoid solvent-containing cutting fluids, which can cause stress cracking.
- Thin walls: the CNC Design Guide gives a 1.5 mm minimum wall and a 3:1 pocket depth-to-width ratio for POM; ABS is more flexible, so treat these values as the floor.
- Internal corners: keep radii at least one-third of the pocket depth. Plastics cannot be EDM-machined, so use corner reliefs where a square part must seat.
- Threads: tapped M2–M10 threads, 1.5–3× the diameter deep, suit occasional assembly; use heat-set inserts for repeated assembly, as the CNC Design Guide recommends for plastics.
- Flatness: large thin plates can bow as stresses in extruded sheet relax; call out flatness only where it matters.
Injection molding ABS
ABS is one of the easiest resins to mold: it flows well, shrinks little (≈ 0.4–0.7%) and gives glossy or textured surfaces straight from the tool. The rules in Uretyco's injection molding DFM guide apply directly:
- Wall thickness: 2.0–2.5 mm recommended, 1.0–4.0 mm as practical limits; keep wall variation under about 25% to avoid sink marks and warpage.
- Draft: at least 1° per side on outside walls and 0.5° or more inside; add about 1° per 0.025 mm of texture depth.
- Ribs and bosses: rib base no more than 60% of the adjoining wall; screw bosses with an outside diameter of about 2× the screw diameter, gusseted if loaded cyclically.
- Gates: at the thickest section, placed so that weld lines and gate marks stay off cosmetic faces.
- Drying: ABS absorbs moisture and must be dried before molding to avoid splay marks on the surface.
FDM printing ABS
ABS is a classic FDM material for functional prototypes and fixtures, but it shrinks as it cools and warps or delaminates without a heated, enclosed build chamber. Printed parts are anisotropic and weakest across the layers (Z), so orient them with the main loads along the layers. Uretyco's 3D printing guide recommends clearance on mating features, test fits before ordering a batch, and inserts or post-machining for threads. Acetone vapor smoothing gives a glossy surface; for UV-exposed printed parts use ASA.
Tolerances and surface finish
For CNC parts, Uretyco treats unspecified tolerances as ISO 2768-mK, with a default surface of about Ra 1.6–3.2 µm and light deburring. Tighter tolerances need a 2D drawing and belong on functional features only; a ±0.025 mm callout on a non-mating face can double the cost. Molded parts follow DIN ISO 20457 (formerly DIN 16742) by default, with SPI finishes from A1 (mirror) to D3 (rough blast). FDM tolerances depend on machine, orientation and size, so test fit-critical features first. Final values are confirmed in the quote and the order.
Finishing options
| Finish | What it adds | Notes for ABS |
|---|---|---|
| As-machined / as-molded / as-printed | Lowest cost | Machined faces show fine tool marks; molded parts copy the tool surface; printed parts show layer lines. |
| Bead blast | Uniform matte look | Hides tool marks on machined parts; typically +5–10% on CNC quotes. |
| Paint | Color, branding | ABS accepts most plastic paints very well after cleaning; mask mating faces and threads. |
| Acetone vapor smoothing (FDM) | Glossy, sealed surface | Removes layer lines; slightly rounds edges and small details. |
| Mold texture | Grip, hides scratches | Defined in the tool; needs extra draft (≈ 1° per 0.025 mm of texture depth). |
ABS is one of the few engineering plastics that bonds readily with solvent cements and most cyanoacrylate, epoxy and acrylic adhesives, so shapes that would be costly as one part can be assembled from several machined or printed parts.
Cost and lead-time drivers
ABS is among the lowest-cost engineering plastics, so on CNC parts the price is set mainly by machining. As a rule of thumb, material is typically 10–30% of a CNC quote, machine time 35–55% and setups 10–20%. The main levers:
- Process by quantity: FDM or CNC for one-offs and small batches; injection molding once the design is frozen and the quantity pays for the tool.
- Tooling: for runs under about 10,000 parts, aluminum tooling is typically 50–65% cheaper than steel and ships in 2–3 weeks; hardened steel pays off from about 25,000 parts.
- Setups: a CNC part made in two setups costs roughly half as much as one that needs four.
- Stock and color: standard black and natural sheet and rod are common; special colors, flame-retardant or other special grades can add lead time.
- Documents: material certificates and inspection reports are opt-in and can extend the lead time. Request them at quote time.
ABS vs. common alternatives
| Material | Impact | Service temperature | UV / outdoor | Chemicals | Relative cost |
|---|---|---|---|---|---|
| ABS | Good | ≈ 60–80 °C | Poor; yellows | Fair; ketones and esters attack it | Baseline |
| ASA | Similar | ≈ 70–85 °C | Very good | Similar to ABS | Slightly higher |
| PC | Very high | ≈ 115–125 °C | Fair; needs UV grade or coating | Poor against solvents (stress cracking) | ≈ 1.5× |
| PETG | Good | ≈ 60–70 °C | Fair to good | Good against many dilute chemicals | Similar |
| POM | Good | ≈ 90–105 °C | Poor; needs UV-stabilized grade | Very good against fuels and solvents | Higher |
For outdoor parts, ASA is the direct substitute: it prints, machines and molds like ABS but resists UV. Step up to PC when impact strength or heat matters more than cost.
When not to choose ABS
Unpainted outdoor or behind-glass parts: use ASA. Continuous service above about 80 °C, or loaded parts near hot electronics: consider PC or PEEK. Contact with acetone, MEK, many fuels or aggressive cleaners: consider POM, PA12 or PEEK. Impact-critical guards: use PC. Food-contact parts: choose a grade with a food-contact declaration and avoid FDM parts, whose layer lines trap residue.
Typical applications
- Indoor housings and enclosures for electronics, instruments and appliances.
- Covers, bezels, knobs and interior trim.
- Look-like and fit-check prototypes before injection tooling.
- Jigs, fixtures and assembly aids (CNC or FDM).
- Toys and household products (molded).
- Painted decorative parts.
Specifying ABS on Uretyco
- 1Choose the process
CNC for small batches and precise features, FDM for fast prototypes, injection molding for stable designs in volume.
- 2Name the grade and color
Standard ABS unless you need flame retardance, higher heat resistance or UV protection (for UV, consider ASA); give color as a RAL code or sample.
- 3Upload STEP plus a 2D drawing
Needed for anything tighter than ISO 2768-mK, threads, inserts or cosmetic requirements; for molding, show parting line, gate preference and textured faces.
- 4Request documents at quote time
Material certificates and inspection reports are opt-in.
FAQ
Can ABS be used outdoors?
Only with protection. Unpainted ABS yellows and loses impact strength under UV within months to a few years, depending on exposure. Paint it, or switch to ASA, which machines and prints like ABS but keeps its color and toughness outdoors.
Are FDM-printed ABS parts as strong as molded ABS?
No. Printed parts contain layer interfaces, voids and infill, so strength is lower than molded or machined ABS, most of all across the layers. Use them for prototypes and fixtures, and validate load-bearing printed parts under real conditions, as Uretyco's 3D printing guide recommends.
Is there an ESD-safe or flame-retardant ABS?
Yes, but they are different grades. Flame-retardant (FR) ABS improves the UL 94 rating; static-dissipative (ESD) ABS contains conductive additives. State the exact requirement in the order notes so the right grade is quoted.
Related resources
- ASAUV-stable alternative for outdoor parts.
- Polycarbonate (PC)When impact or heat matters more than cost.
- PETGEasy-to-print alternative with low warp.
- Engineering Plastics ComparedABS, PC, PEEK and PA12 side by side.
- Injection Molding DFMWalls, draft, ribs, gates and tooling.
- CNC Design GuideTolerances, walls, threads and setups.
- 3D PrintingChoosing between FDM, SLA, SLS and MJF.
- Technical Drawings & TolerancesWhat belongs on the 2D drawing.
Related materials