PEEK (polyether ether ketone) is a semi-crystalline, high-performance thermoplastic. It keeps useful properties up to about 250 °C, resists almost all common chemicals as well as hot water and steam, wears well, and is inherently flame-retardant with low smoke emission. Unfilled PEEK is tough and ductile; glass- and carbon-filled grades add stiffness and heat resistance.
Choose PEEK when no lower-cost plastic survives the temperature, chemicals or sterilization cycles, or when a polymer must replace metal for weight, insulation or corrosion reasons. It is not a default material: raw stock costs roughly 10–15× ABS. On Uretyco it is offered for CNC machining, injection molding and FDM printing.
Mechanical and physical properties
| Property | Typical value | Notes |
|---|---|---|
| Tensile strength | ≈ 95–115 MPa | Unfilled. Glass- and carbon-filled grades are considerably stronger. |
| Elongation at break | ≈ 15–45% | Unfilled; filled grades only ≈ 1–3%. |
| Tensile modulus | ≈ 3.6–4.2 GPa | Filled grades are roughly 3–6× stiffer. |
| Density | ≈ 1.30–1.32 g/cm³ | Filled grades ≈ 1.4–1.5 g/cm³; about half the density of aluminum. |
| Glass transition (Tg) | ≈ 143 °C | Stiffness drops noticeably above Tg; filled grades retain more of it. |
| Melting point | ≈ 343 °C | Semi-crystalline: no gradual softening below the melt. |
| Heat deflection temperature (HDT) | ≈ 150–160 °C | At 1.8 MPa, unfilled; ≈ 300 °C or more for 30% glass- or carbon-filled grades. |
| Max. continuous service temperature | ≈ 250–260 °C | Thermal-ageing rating. For loaded parts above Tg, use filled grades and check creep data. |
| Thermal expansion | ≈ 45–55 µm/m·K | Below Tg, about twice aluminum; more than doubles above Tg. Much lower along the fibers in filled grades. |
| Water absorption | ≈ 0.1–0.5% | 24 h to saturation; dimensionally stable in humid environments. |
| Flammability | UL 94 V-0 | Without additives, at about 1.5 mm; low smoke and toxic-gas emission. |
Typical room-temperature values for unfilled PEEK. Extruded stock shapes and molded parts differ, and filled, bearing and medical grades differ further. For design calculations, use the data sheet of the specific grade named in your quote.
CNC machining PEEK
PEEK cuts cleanly with sharp carbide tools, but it needs more care than its reputation suggests: scrap is expensive, the material is heat-sensitive, and internal stresses can move a part after machining. Glass- and carbon-filled grades are abrasive. Watch for:
- Stress and stability: use annealed (stress-relieved) stock and, for tight tolerances, rough-machine, anneal, then finish. Thick rod and plate can release stress as material is removed.
- Heat and tools: keep tools sharp and use coolant or air; overheated PEEK smears and builds surface stress. Carbide is standard; for longer runs in filled grades, diamond-coated or PCD tools last far longer.
- Walls and corners: start from the CNC Design Guide's plastic values (1.5 mm minimum wall and 3:1 pocket depth-to-width for POM) and keep internal radii at least one-third of the pocket depth. Filled grades are brittle, so avoid sharp notches.
- Threads: tapped M2–M10 threads, 1.5–3× the diameter deep, work well in unfilled PEEK; for repeated assembly or filled grades, use threaded inserts.
Injection molding PEEK
PEEK follows standard molding DFM but at much higher temperatures: melt temperatures around 360–400 °C and mold temperatures around 170–200 °C are typical, so that the part crystallizes properly. That narrows the supplier pool and makes tool choice important; Uretyco's quoting engine weighs tooling by volume and by how aggressive the material is. Key rules from the injection molding DFM guide:
- Wall thickness: the guide's general sweet spot of 1.5–3.5 mm applies; keep wall variation under about 25%.
- Draft: at least 1° per side outside and 0.5° or more inside; add about 1° per 0.025 mm of texture depth.
- Ribs and bosses: rib base no more than 60% of the wall; bosses about 2× the screw diameter outside, gusseted under cyclic load.
- Filled grades: fibers orient with the flow, so shrinkage and strength differ along and across it; place gates and weld lines with this in mind.
FDM printing PEEK
PEEK can be printed by FDM on high-temperature machines with heated chambers. It suits one-off brackets, fixtures and test parts that must see PEEK's temperature or chemical environment. Printed parts are weaker across the layers, and their crystallinity, and with it stiffness and heat resistance, depends on the printer and on annealing after printing. Treat printed PEEK as a prototype or low-volume option and, as Uretyco's 3D printing guide advises, validate load-bearing parts in their real environment.
Tolerances and surface finish
For machined PEEK, Uretyco treats unspecified tolerances as ISO 2768-mK, with a default surface of about Ra 1.6–3.2 µm and light deburring; tighter tolerances need a 2D drawing and belong on functional features only. PEEK holds tight tolerances well when the stock is annealed and the part is finished after stress relief, but it expands about twice as much as aluminum, so state the inspection temperature for precision fits. Molded parts follow DIN ISO 20457 (formerly DIN 16742) by default. Final values are confirmed in the quote and the order.
Finishing options
PEEK is usually used as-machined: it needs no corrosion protection and is hard to paint or bond. Typical options:
| Finish | What it adds | Notes for PEEK |
|---|---|---|
| As-machined | Lowest cost | Natural beige or black; clean, slightly glossy faces. |
| Bead blast | Uniform matte look | Hides tool marks; typically +5–10% on CNC quotes. |
| Polished functional faces | Sealing and sliding surfaces | Specify Ra only where needed; mirror polish (Ra < 0.4 µm) typically +50–150% on CNC quotes. |
| Painting or bonding | Rarely needed | Requires surface activation (e.g. plasma); prefer mechanical fastening. |
Cost and lead-time drivers
Material is a much larger share of a PEEK part than of an ABS or aluminum part, so scrap and the ratio of stock bought to finished part weight matter. The main levers:
- Stock size: design parts to fit standard rod and plate sizes, and avoid machining small parts from thick plate. High-performance plastics can cost more and need longer lead times, as Uretyco's material selection guide notes.
- Grade: unfilled natural is the most available; carbon-filled, glass-filled, bearing and medical grades are specialty items with longer lead times.
- Tolerances: tight tolerances may require annealing between roughing and finishing, which adds a step and time.
- Documents: material certificates and traceability are opt-in and can extend the lead time. Request them at quote time, especially for regulated applications.
PEEK vs. common alternatives
| Material | Max. continuous use | Chemical resistance | Machinability | Relative cost |
|---|---|---|---|---|
| PEEK | ≈ 250 °C | Excellent, incl. hot water and steam | Good, with care | Baseline (stock ≈ 10–15× ABS) |
| PEI (e.g. Ultem) | ≈ 170 °C | Good; attacked by some solvents | Good | Lower |
| PPS | ≈ 200–220 °C | Excellent | Fair; unfilled grade is brittle | Lower |
| POM | ≈ 90–105 °C | Very good against fuels and solvents; poor against strong acids | Excellent | Much lower |
| Aluminum 6061-T6 | ≈ 100–150 °C | Good; attacked by strong acids and alkalis | Excellent | Much lower |
If the requirement is a temperature below about 170 °C without aggressive chemicals, PEI is often enough; if the part only needs low friction and stiffness at moderate temperature, POM costs a fraction of PEEK. PEEK earns its price above roughly 200 °C, in steam or aggressive media, and where a metal must be replaced by a light, insulating polymer.
When not to choose PEEK
Cost-driven parts that only need moderate temperature or low friction: use POM, PA or PEI. Concentrated sulfuric or nitric acid: these attack PEEK. Highly loaded structural parts above Tg (143 °C) in unfilled grade: use a filled grade or metal. Implants with standard PEEK: implant-grade material qualified to ASTM F2026 and a regulated supply chain are required. Long outdoor UV exposure without protection: natural PEEK has limited UV resistance.
Typical applications
- Seals, back-up rings, valve seats and pump parts in aggressive media.
- Bearings, bushings, thrust washers and wear pads (bearing grades).
- Semiconductor and wafer-handling components.
- High-temperature electrical insulators and connectors.
- Aerospace and automotive brackets, clips and fluid-system parts.
- Medical instrument components that see repeated sterilization (medical grades).
Specifying PEEK on Uretyco
- 1Select PEEK and the process
CNC for most parts and small batches, injection molding for stable designs in volume, FDM for test parts.
- 2Name the grade
Unfilled natural or black, 30% glass, 30% carbon, bearing or medical grade: state it in the order notes so availability is confirmed in the quote.
- 3Upload STEP plus a 2D drawing
Mark tight tolerances, sealing faces and threads; note if annealing between roughing and finishing is required.
- 4Request documents at quote time
Material certificates and traceability are opt-in; for medical or regulated use, request the documents your process requires.
FAQ
Can standard PEEK be used for implants?
No. Implantable devices require implant-grade PEEK qualified to ASTM F2026, with the material supplier's regulatory documentation and a controlled supply chain. Standard industrial PEEK suits instruments and device housings, not implantation. State the intended use and the documents you need in the order notes; whether the part suits it is your decision and your responsible engineer's.
Unfilled, glass-filled or carbon-filled PEEK?
Unfilled PEEK is the toughest and the right choice for parts that must flex or take impact. 30% glass-filled adds stiffness and dimensional stability; 30% carbon-filled is stiffer still, lighter and better in wear. Bearing grades combine carbon fiber, graphite and PTFE for low friction. Filled grades are more brittle and wear tools faster.
Is PEEK really as easy to machine as aluminum?
It cuts cleanly, but it is not a drop-in replacement. It holds internal stresses, is sensitive to heat, and scrap is expensive. Annealed stock, sharp tools and, for tight tolerances, a stress-relief step between roughing and finishing give the best results.
Related resources
- Delrin / POM (Acetal)Low-cost choice for low friction at moderate temperature.
- Polycarbonate (PC)Tough, transparent, up to about 125 °C.
- Aluminum 6061-T6When metal strength is acceptable.
- Engineering Plastics ComparedABS, PC, PEEK and PA12 side by side.
- CNC Design GuideTolerances, walls, threads and setups.
- Injection Molding DFMWalls, draft, ribs, gates and tooling.
- Material Selection GuideStart from the requirement, not the material name.
- Quality Control & InspectionCertificates, reports and inspection scope.
Related materials
Can't find what you need? Contact our team for expert assistance with your manufacturing project.