Titanium Grade 5 (Ti-6Al-4V, UNS R56400, material number 3.7165) is an alpha-beta titanium alloy with 6% aluminum and 4% vanadium, and the most widely used titanium alloy. Annealed, it matches the tensile strength of quenched and tempered alloy steel at about 56% of the density, resists corrosion outstandingly, including in seawater, and keeps useful strength up to about 400 °C.
Choose it when strength-to-weight, corrosion resistance or temperature rule out aluminum and stainless steel: aerospace and motorsport fittings, marine and chemical hardware, and medical instruments. Stock costs several times as much as aluminum and machining is slow, so it is rarely the economical choice unless the application needs it. Besides CNC machining, Ti-6Al-4V can be requested through Uretyco for metal 3D printing by laser powder bed fusion, electron beam melting or DED.
Mechanical and physical properties
| Property | Typical value | Notes |
|---|---|---|
| Tensile strength (Rm) | ≈ 950–1000 MPa | Annealed; specification minimum 895 MPa (ASTM B348 bar). Solution-treated and aged material is stronger. |
| Yield strength (Rp0.2) | ≈ 880 MPa | Minimum 828 MPa (ASTM B348); high yield-to-tensile ratio, so little reserve after yielding. |
| Elongation at break | ≈ 10–14% | Minimum 10%. |
| Hardness | ≈ 33–36 HRC | ≈ 330–350 HV. |
| Elastic modulus | ≈ 114 GPa | About half of steel; titanium parts deflect and spring back more, both in cutting and in service. |
| Density | 4.43 g/cm³ | ≈ 56% of steel, ≈ 1.6× aluminum. |
| Thermal conductivity | ≈ 6.7 W/m·K | Less than half of stainless 304; heat stays at the cutting edge. |
| Thermal expansion | ≈ 8.6 µm/m·K | Lower than steel and far lower than aluminum. |
| Electrical conductivity | ≈ 1% IACS | Poor conductor. |
| Magnetic behavior | Non-magnetic | Suitable near sensors. |
| Service temperature | Up to ≈ 400 °C | Strength holds well to ≈ 400 °C; above that, oxidation and loss of strength limit use. |
Typical room-temperature values for annealed wrought Ti-6Al-4V bar and plate; values vary with product form, section size and heat treatment. For calculations, use the minimums of the governing standard (e.g. ASTM B348/B265, AMS 4911/4928) or your material certificate.
Machining Ti-6Al-4V
Titanium is not difficult because it is as hard as hardened steel. It is difficult because heat does not leave through the chip or the part, and because the metal reacts with and sticks to the tool. Low cutting speeds, a high feed per tooth, sharp coated carbide, constant tool engagement, high-pressure coolant and very rigid fixturing are standard. Watch for:
- Thin walls and deflection: with about half the stiffness of steel, thin walls and long features chatter and spring away from the cutter. The CNC Design Guide gives no titanium-specific minimum wall; design generous walls and ribs, and check the DFM findings for thin features.
- Heat and tool life: cutting speeds are a fraction of those used for aluminum, so machine time, not stock, is usually the largest cost. Avoid deep, narrow pockets and small cutters where possible.
- Internal corners: keep radii at least one-third of the pocket depth, and larger where you can, so that bigger, stiffer tools can be used.
- Threads: use standard sizes (M2–M10), 1.5–3× the diameter deep. Titanium threads gall easily against titanium or stainless; use anti-seize, anodized or coated fasteners, or thread inserts.
- Chips and safety: fine titanium chips and dust can ignite, so coolant and chip handling matter more than with steel.
Tolerances and surface finish
Uretyco treats unspecified tolerances as ISO 2768-mK, with a default as-machined surface of around Ra 1.6–3.2 µm and light deburring. Tight tolerances cost more machine time in titanium than in aluminum or steel, so keep them to functional features and put them on a 2D drawing. Surface condition strongly affects titanium's fatigue life; state Ra on fatigue-critical surfaces. Final values are confirmed in the quote and the order.
Finishing options
Ti-6Al-4V needs no coating for corrosion protection: its natural oxide film makes it resistant to seawater, chlorides and most chemicals. Finishes are used for appearance, identification, wear and galling resistance, or surface preparation.
| Finish | What it adds | Notes for Ti-6Al-4V |
|---|---|---|
| As-machined | Lowest cost | Grey metallic surface; fully corrosion-resistant without treatment. |
| Bead blast | Uniform matte look | Hides tool marks; use clean, iron-free media. Often done before anodizing. |
| Color anodizing (AMS 2488 Type 3) | Interference colors without dye | Thin oxide whose color depends on voltage (gold, blue, purple, green); used for identification and appearance. Negligible dimensional change. |
| Anti-galling anodizing (AMS 2488 Type 2) | Galling and wear resistance | Grey oxide layer that reduces galling on threads and sliding contacts. |
| Pickling | Clean, uniform surface | Removes contamination and oxide; common before welding or bonding. |
| Polish / electropolish | Smooth surface | Improves cleanability and fatigue-critical surfaces; specify the target Ra. |
Titanium galls against itself and against stainless steel, so threaded or sliding joints need anti-seize, anti-galling anodizing or a different counterpart material. Titanium is also noble: in wet conditions, aluminum or carbon steel touching it will corrode, so isolate the contact.
- Surface Finish GuideFinishes and drawing callouts.
- Surface FinishingProcess overview, masking and quality notes.
Cost and lead-time drivers
As a rule of thumb, material is typically 10–30% of a CNC quote, machine time 35–55% and finishing 0–25%. With expensive stock, slow cutting and fast tool wear, titanium sits near the top of the material and machine-time ranges. Rare alloys and certified batches may also cost more and need a longer lead time. The main levers:
- Material utilization: with expensive stock, start from bar or plate close to the final shape; turning 90% of a large block into chips is costly.
- Geometry: thicker walls, larger radii, shallow pockets and fewer setups save more machine time in titanium than in aluminum or steel. A part machined in two setups costs roughly half of one that needs four.
- Grade and certification: Grade 5 bar and plate are widely stocked; Grade 23 ELI, certified aerospace or medical material and unusual sizes add time.
- Documents: material certificates and inspection reports are opt-in and can extend the lead time. For traceable aerospace or medical parts, request them at quote time.
Ti-6Al-4V vs. common alternatives
| Material | Strength | Density | Corrosion | Machinability | Relative cost |
|---|---|---|---|---|---|
| Ti-6Al-4V (Grade 5) | Baseline (Rm ≈ 950 MPa) | 4.43 g/cm³ | Excellent | Difficult | Baseline |
| Titanium Grade 2 (CP) | ≈ 35–45% (Rm ≥ 345 MPa) | 4.51 g/cm³ | Excellent; best in chemical service | Fair | Lower |
| Aluminum 7075-T6 | ≈ 60% (Rm ≈ 570 MPa) | 2.81 g/cm³ | Fair; needs protection | Good | Much lower |
| Stainless 17-4 PH | Similar to higher (Rm ≈ 1000–1300 MPa) | ≈ 7.8 g/cm³ | Good | Fair | Lower |
| Stainless 316L | ≈ 50–70% (Rm ≈ 485–680 MPa) | 8.0 g/cm³ | Very good; limited in seawater crevices | Fair | Much lower |
| Inconel 718 | Higher (Rm ≈ 1240 MPa); strong to ≈ 700 °C | 8.19 g/cm³ | Excellent | Very difficult | Higher |
Per unit weight, Ti-6Al-4V comfortably beats 17-4 PH and 316L and edges out 7075-T6, while adding corrosion and temperature resistance that aluminum cannot match. If weight is not critical, 17-4 PH is usually cheaper for the same strength; if only corrosion matters, Grade 2 or 316L may be enough.
When not to choose Ti-6Al-4V
Cost-driven parts whose load 6061 or 7075 could carry: titanium can multiply the part price. Stiffness-limited parts: its modulus is only about half of steel's, so a steel part of the same size deflects less. Sliding or threaded contact without anti-galling measures: titanium galls. Service above ≈ 400 °C: consider Inconel 718. Surgical implants: these require implant-grade Ti-6Al-4V ELI (Grade 23, ASTM F136), full traceability and a regulatory approval route; state the intended use and the documents you need in the order.
Typical applications
- Aerospace and UAV fittings, brackets and fasteners.
- Motorsport and cycling components where weight and fatigue matter.
- Marine, offshore and chemical-process hardware exposed to seawater or chlorides.
- Medical instruments and non-implant device components.
- Parts near engines and exhausts operating up to ≈ 400 °C.
- Lightweight, non-magnetic parts for instruments and robotics.
Specifying titanium Grade 5 on Uretyco
- 1Select Ti-6Al-4V Grade 5 and the condition
Annealed is standard; state Grade 23 ELI, solution-treated and aged material, or a specific standard (for example AMS 4928) if required.
- 2Upload STEP plus a 2D drawing
Mark tolerances tighter than ISO 2768-mK, Ra on fatigue-critical surfaces, threads, anodize color and masked areas.
- 3Request documents at quote time
Material certificates and traceability are opt-in, not automatic; aerospace and medical projects should request them before production.
FAQ
What is the difference between Grade 5 and Grade 23?
Grade 23 (Ti-6Al-4V ELI, extra-low interstitial) limits oxygen and iron more tightly. Its strength is slightly lower, but toughness and fatigue behavior are better, and it is the standard alloy for surgical implants (ASTM F136). For general engineering parts, Grade 5 is the usual choice.
Grade 5 or Grade 2?
Grade 2 is commercially pure titanium: about 40% of the strength of Grade 5, but easier to form and weld, and slightly better in some chemical environments. Choose Grade 2 for lightly loaded, corrosion-driven parts and Grade 5 when strength matters.
Can titanium be anodized in colors?
Yes. Color anodizing grows a thin, transparent oxide whose thickness, set by the voltage, produces interference colors such as gold, blue, purple and green without dyes. Colors are repeatable for a given process but vary slightly with surface finish, so approve a sample for cosmetic parts. The process differs from aluminum anodizing and adds no meaningful thickness.
Is titanium stronger than steel?
Grade 5 is about as strong as quenched and tempered alloy steels such as 4140 at about 56% of the weight, so it is far stronger per kilogram. It is not stiffer, though: its modulus is about half of steel's, and it is not harder than hardened steel. For wear surfaces, hardened steel or a coating is still the better choice.
How do EBM and DED compare with laser powder bed fusion?
All three build Ti-6Al-4V layer by layer, but they suit different parts. Laser powder bed fusion (DMLS, SLM) gives the finest features and the smoothest printed surfaces, typically Ra ≈ 5–15 µm, but parts carry high residual stress, so they are stress-relieved on the build plate and often HIPed for fatigue-critical use. Electron beam melting (EBM) melts the powder in a vacuum with the bed held at about 600–700 °C, so residual stress and oxygen pickup stay low; it is common for implants in Ti-6Al-4V ELI (Grade 23) with porous lattice surfaces, at the cost of rougher surfaces, typically Ra ≈ 20–35 µm, and coarser detail. Directed energy deposition (DED) melts wire or powder with a laser, electron beam or arc and builds large preforms close to final shape, with a machining allowance of a few millimeters on every functional face; compared with machining from a large billet, this saves much of the expensive stock. EBM and DED are specialized routes, so availability and heat treatment are confirmed in the quote. For implants, compliance depends on the certified grade, process validation and the customer's own regulatory approval route.
Related resources
- Aluminum 7075-T6Lower-cost high-strength aluminum.
- Stainless Steel 17-4 PHHigh-strength stainless at lower cost.
- Stainless Steel 316LCorrosion-resistant stainless for less demanding service.
- Inconel 718For service above ≈ 400 °C.
- Alloy Steel 4140Hardenable steel when weight is not critical.
- 3D PrintingMetal printing for complex geometry.
- CNC Design GuideTolerances, walls, threads and setups.
- CNC MachiningProcess overview, files and cost drivers.
- Quality Control & InspectionInspection scope, reports and certificates.
Related materials
Can't find what you need? Contact our team for expert assistance with your manufacturing project.