Liquid silicone rubber (LSR) is a two-component, platinum-catalysed (addition-cure) silicone. The low-viscosity components are mixed 1:1, injected cold into a heated mold and cured in seconds, giving highly repeatable elastomer parts. Silicone keeps its elasticity over a wide temperature range, resists ozone, UV and weathering, and is inert enough to be offered in food-contact and medical grades.
Choose LSR for flexible parts in volume: seals, gaskets, O-rings, membranes, valves, keypads and wearable or baby-care parts, especially where heat, outdoor exposure, sterilization or skin and food contact matter. For prototypes and low volumes, RTV-cast or compression-molded silicone avoids the cost of an LSR injection tool.
Mechanical and physical properties
| Property | Typical value | Notes |
|---|---|---|
| Hardness | Shore 10–80A | Most parts use 30–70A; specify the target value and tolerance, commonly ±5 points. |
| Tensile strength | ≈ 6–11 MPa | Lower than polyurethane or TPU elastomers. |
| Elongation at break | ≈ 200–700% | Softer grades stretch more. |
| Tear strength | ≈ 20–50 kN/m | ASTM D624 die B; high-tear grades for thin membranes. |
| Compression set | ≈ 10–30% | 22 h at 175 °C, post-cured; lower is better for seals. |
| Density | ≈ 1.10–1.20 g/cm³ | Rises with hardness and filler content. |
| Service temperature | ≈ −50 to +200 °C | Special grades extend the range; long exposure near the upper limit hardens the rubber. |
| Linear shrinkage | ≈ 2–4% | High because the mold runs hot; depends on grade, geometry and post-cure. |
| Dielectric strength | ≈ 20–25 kV/mm | Good electrical insulator. |
Typical datasheet values for standard LSR grades after post-cure; actual values depend on the grade, hardness, part geometry and cure. Design seals with the specific grade's data and test them in the real medium and temperature.
Molding LSR
LSR runs differently from thermoplastics: the material is cold and liquid, the mold is hot, and the very low viscosity fills thin sections but also any gap in the tool. Uretyco's silicone-molding guidance, plus common LSR practice:
- Hardness and tear targets: silicone stiffness spans an enormous range, so specify Shore hardness and tear strength, with tolerances, on the drawing.
- Radii and demolding: avoid sharp internal corners; generous radii reduce tearing during demolding. LSR's elasticity allows undercuts and little or no draft that would lock a thermoplastic part.
- Gate vestiges and flash: plan where gate marks and parting lines fall and map cosmetic surfaces relative to the tool splits. LSR flashes into gaps of only a few micrometres, so shut-offs on sealing faces matter.
- Shrinkage: validate shrink separately from plastics; silicone behaves unlike thermoplastic melts and shrinks more.
- Walls: LSR fills thin membranes and keypad webs well and tolerates wall changes better than thermoplastics, but thick sections lengthen cure time.
- Overmolding: self-adhesive grades bond to selected thermoplastics or metals in two-shot or insert molding; adhesion must be validated.
- Post-cure: many food-contact and medical applications require post-curing in an oven to remove volatiles and improve compression set; state it on the drawing.
Prototype and low-volume silicone
Before an LSR tool is justified, silicone parts can be RTV-cast in soft tools or compression-molded, a route commonly used for gaskets. Uretyco's guide sums it up: LSR suits higher volumes and tighter repeats, RTV suits prototyping and low volumes. Properties, surface and repeatability differ from LSR, so validate critical seals in the production grade before release.
Tolerances and surface
Once the tool is right, LSR parts repeat closely. Absolute tolerances depend on shrinkage, part size and hardness and are confirmed in the quote and the order. Soft parts also deform under the measuring force, so define how critical dimensions are measured. The surface copies the tool: polished for clear or glossy parts, textured or blasted to reduce tackiness and hide flow marks.
Finishing and secondary operations
LSR parts usually ship as molded. Typical secondary steps:
| Operation | Purpose | Notes |
|---|---|---|
| Deflashing and trimming | Remove flash and gate vestiges | Manual or cryogenic; minimized by good tool shut-offs. |
| Post-curing | Fewer volatiles, better compression set | Often required for food-contact and medical grades; adds oven time. |
| Surface coating | Lower tack and friction | Helps assembly and the feel of soft parts. |
| Printing and marking | Logos, legends | Needs silicone-specific inks; adhesion is harder than on plastics. |
| Pigmentation | Color | Natural LSR is translucent; colors are added as masterbatch. |
Food-contact and medical suitability belongs to a specific grade and its processing, including post-cure, not to silicone in general. Name the required standard or approval in the order and request the supplier's declaration or certificate at quote time.
- Silicone MoldingLSR, RTV and soft-tool silicone workflows.
- Injection MoldingTooling economics and tolerance notes.
Cost and lead-time drivers
LSR has a low cost per part at volume but needs a demanding tool.
- Tooling: LSR molds need precise shut-offs, venting and heating to control flash; cavity count and automation set the investment.
- Prototype path: RTV casting or compression molding avoids the LSR tool for early quantities. Uretyco compares silicone routes and injection molding based on quantity, tolerance and cosmetic goals.
- Material and grade: LSR costs more per kilogram than commodity thermoplastics; medical, food-contact, optical and self-adhesive grades cost more again.
- Secondary operations: deflashing, post-curing and coating add cost and lead time.
- Documents: inspection reports, material certificates and first-article approval are opt-in; request them at quote time.
LSR vs. common alternatives
| Material and route | Temperature range | Tear and abrasion | Food or medical grades | Tooling and volume |
|---|---|---|---|---|
| LSR (injection) | ≈ −50 to +200 °C | Moderate | Yes, grade-specific | High tooling cost; high volumes |
| HCR silicone (compression) | Similar | Moderate to good | Yes, grade-specific | Lower tooling cost; low to medium volumes |
| RTV-cast silicone | Similar | Lower | Limited | Lowest tooling cost; prototypes |
| TPU 95A | Narrower; upper limit ≈ 80–100 °C | Very good | Some grades | Injection molding or 3D printing |
| Cast polyurethane elastomer | Narrower | Good | Rarely | Low tooling cost; up to about 200 parts |
Silicone's weak points are tear and abrasion resistance and swelling in oils and fuels. Uretyco's silicone guide notes that silicone can sometimes replace TPU for temperature or chemical resistance, but its mechanical damping differs; where abrasion or tear loads dominate, TPU or polyurethane is usually better, and fluorosilicone is used for fuel contact.
When not to choose LSR
Immersion in fuels or mineral oils: use fluorosilicone or a fluoroelastomer. Abrasive wear or high tear loads: use polyurethane or TPU. Very low quantities where an LSR tool will not pay back: use RTV or compression molding. Rigid or load-bearing parts. Gas-tight membranes: silicone is highly permeable to gases.
Typical applications
- Seals, gaskets and O-rings.
- Medical masks, valves and device seals.
- Baby-care and kitchen products.
- Keypads, wearable straps and soft-touch covers.
- Connector seals and automotive boots.
- LED lenses and light guides in optical grades.
Specifying LSR on Uretyco
- 1Specify grade and hardness
Shore A value with tolerance, color, and any food-contact, medical or flame-retardant requirement by name.
- 2Upload STEP plus a drawing
Show sealing faces, allowed parting-line and gate areas, critical dimensions with the measurement method, and post-cure requirements.
- 3Plan prototypes and first articles
Validate with RTV or prototype-tool parts, then request first-article approval and documents at quote time.
FAQ
LSR or RTV silicone?
LSR suits higher volumes and tighter repeats; RTV suits prototyping and low volumes. A common path is RTV or compression-molded parts for validation, then an LSR tool once the design and quantities are stable.
Is LSR food-safe and biocompatible?
Specific grades are formulated and tested for food contact (for example FDA 21 CFR 177.2600 or BfR Recommendation XV) or for biocompatibility (ISO 10993 or USP Class VI testing), usually combined with post-curing. Compliance belongs to the grade and the finished part, and for medical devices the device manufacturer remains responsible for validation.
Can silicone replace TPU?
Sometimes, mainly for temperature or chemical resistance, but mechanical damping, tear and abrasion behave differently. Silicone stays flexible from deep cold to about 200 °C; TPU is tougher against wear and tearing at moderate temperatures.
Can LSR parts be clear or colored?
Yes. Natural LSR is translucent, optical grades are highly transparent, and pigments give solid colors matched to RAL, Pantone or a sample. Expect small shade differences between batches and state color tolerance for visible parts.
Related resources
- Silicone MoldingLSR, RTV and soft-tool silicone workflows.
- Molding & Casting OverviewShared files, design themes and tolerance notes.
- Injection MoldingTooling economics and tolerance notes.
- Cast PolyurethaneLow-volume elastomer and rigid parts.
- TPU 95AWear-resistant thermoplastic elastomer.
- Bridge ProductionPlanning the step from prototype to volume.
- Quality Control & InspectionFirst article, reports and certificates.
- Technical Drawings & TolerancesWhat belongs on the 2D drawing.
Related materials
Can't find what you need? Contact our team for expert assistance with your manufacturing project.