Cast polyurethane is a family of two-part resins (isocyanate plus polyol) that are mixed, degassed and poured into a silicone (RTV) mold, usually under vacuum, then cured with heat. By changing the formulation, the same process makes soft elastomers around Shore 30A, rubber-like parts, and rigid plastics up to about Shore 85D that imitate ABS, PP, PC or PMMA, including clear, colored, flame-retardant and high-temperature grades.
Choose it when you need tens of parts that look and feel like production plastic or rubber before tooling is justified: marketing samples, pilot builds, field-test units and small batches. Uretyco's bridge-production article places cast urethane at up to about 200 parts, with low tooling cost, high per-part cost and first parts in 1–2 weeks.
Grades and typical properties
| Grade family | Hardness | Tensile strength | Elongation at break | Typical use |
|---|---|---|---|---|
| Soft elastomer | Shore 30–60A | ≈ 2–8 MPa | ≈ 300–600% | Gaskets, grips, soft-touch covers |
| Medium elastomer | Shore 70–95A | ≈ 8–25 MPa | ≈ 200–500% | Bumpers, seals, wheels, overmold simulation |
| Semi-rigid (PP-like) | Shore 65–75D | ≈ 20–35 MPa | ≈ 20–100% | Clips, flexible housings, snap fits |
| Rigid (ABS-like) | Shore 75–85D | ≈ 40–65 MPa | ≈ 5–20% | Housings, covers, trim |
| Clear (PMMA/PC-like) | Shore 80–87D | ≈ 50–75 MPa | ≈ 5–15% | Lenses, light guides, transparent covers |
Unfilled grades have a density of about 1.05–1.20 g/cm³. Standard rigid grades have heat deflection temperatures of roughly 60–90 °C; dedicated high-temperature and flame-retardant formulations exist for parts near heat sources or with flammability targets.
Values vary by resin brand, grade, mix ratio, cure schedule and wall thickness. 'ABS-like' or 'PP-like' means similar hardness and stiffness, not the same chemical resistance, aging, UV stability or certifications as the thermoplastic. Design with the specific resin datasheet and validate parts in their real environment.
Vacuum casting in silicone molds
The process starts from a master pattern, usually an SLA or PolyJet print or a machined part, finished to the surface the cast parts should have. Silicone is poured around the master, the mold is cut open along a planned parting line, and resin is cast into it. Typical design guidance:
- Master quality: every scratch, layer line and sanding mark on the master transfers to every part, so specify texture or gloss for the master.
- Walls: uniform walls of roughly 1.5–3 mm cast most reliably; very thin or very thick sections risk short fills, sink or distortion.
- Undercuts and corners: the flexible silicone tolerates undercuts and little draft, but sharp internal corners tear the mold. Uretyco's silicone-molding guidance recommends generous radii and planning where parting lines, gate marks and flash will fall.
- Inserts: threaded inserts can be cast in place or installed afterwards; list them with the drawing.
- Large flat parts: thin, large panels can warp during cure; ribs or a slightly thicker wall help.
Tolerances and surface
Cast-urethane accuracy depends on the master, mold and resin shrinkage, and part size; it is confirmed in the quote and the order. Put critical fits on a drawing, expect more variation than with injection molding, and validate assemblies with the first parts. The surface follows the master: a polished master gives glossy parts, a bead-blasted one a uniform matte texture.
Color and finishing
Most finishing happens in the resin or on the master rather than on each part.
| Option | What it adds | Notes |
|---|---|---|
| In-mass color | Color through the part | Pigment matched to RAL, Pantone or a sample; slight shade variation between batches. |
| Master texture | Matte, gloss or textured surface | Applied to the master before mold making and copied to every part from that mold. |
| Painting, soft-touch paint | Exact color, haptics | The most consistent color match; needs good surface preparation. |
| Clear grades, polished | Transparency | Clear parts can yellow with UV exposure over time; protect or test them. |
| Pad printing | Logos, legends | Applied after painting where required. |
Soft and rigid urethanes can be cast in sequence into one part to imitate overmolded or two-shot production parts. That makes cast urethane a practical way to test grips and seals before investing in two-shot tooling.
- Silicone MoldingRTV, LSR and soft-tool silicone workflows.
- Bridge ProductionWhere cast urethane fits between prototype and volume.
Cost and lead-time drivers
Cast urethane trades low tooling cost for a higher price per part.
- Master: a printed and hand-finished master is the first cost item; reusing an existing master saves time.
- Molds: each silicone mold yields a limited number of parts, so cost steps up with every extra mold; size and complexity set mold cost.
- Resin and labor: special grades (clear, high-temperature, flame-retardant), painting and inserts add cost, and per-part cost falls only slowly with quantity.
- Lead time: Uretyco's bridge-production article puts first parts at about 1–2 weeks; color matching, painting and inspection scope add time.
- Documents: inspection reports and first-article approval are opt-in and should be requested at quote time.
Cast urethane vs. other bridge options
| Option | Best for | Tooling cost | Per-unit cost | Lead time to first part |
|---|---|---|---|---|
| Cast urethane (RTV) | ≤ 200 parts | Low | High | 1–2 weeks |
| MJF / SLS | ≤ 5,000 nylon parts | None | Medium | 5–10 days |
| Soft (aluminum) injection tooling | 1,000–25,000 parts | Low | Low-medium | 2–3 weeks |
| Hard (steel) injection tooling | 25,000+ parts | High | Lowest | 6–10 weeks |
These figures come from Uretyco's bridge-production article. Material realism differs too: MJF parts are real nylon, injection-molded parts are the production material, and cast urethane imitates the target plastic. For flexible parts in higher volumes, or in medical, food-contact or high-temperature service, LSR or another silicone route is the stronger choice.
When not to choose cast polyurethane
Quantities beyond a few hundred parts: mold life and labor keep per-part cost high. Parts that must be tested in the specified production material (UL listings, food contact, medical): use the real material. Long-term outdoor exposure without paint, or service above the resin's heat limit. Tight tolerances across large parts. Exposure to fuels, solvents or other aggressive chemicals.
Typical applications
- Look-and-feel prototypes and marketing samples.
- Pilot builds, field-test units and small production batches.
- Low-volume housings, covers and trim.
- Soft-touch grips, gaskets, seals and bumpers.
- Clear lenses and light-guide prototypes.
- Simulations of overmolded and two-shot parts.
Specifying cast polyurethane on Uretyco
- 1Choose the resin by function
Give the target hardness (Shore A or D), the plastic or rubber it should imitate, the color (RAL, Pantone or sample) and any clear, heat or flame-retardant requirement.
- 2Upload STEP plus a drawing
Show critical dimensions, visible faces, texture, inserts and acceptable parting-line and gate locations.
- 3Approve first parts
For pilot batches, request first-article or sample approval before the full run; it is opt-in.
FAQ
How many parts can one silicone mold make?
Typically around 15–25, depending on resin, geometry and surface demands; aggressive resins, deep undercuts and glossy cosmetic surfaces shorten mold life. Larger quantities use several molds made from the same master.
Why not just 3D print the parts?
For a handful of parts, printing is usually faster and cheaper. Cast urethane pays off when you need tens of identical parts with a molded-looking surface, through-color, clear sections or rubber-like grades that printing does not offer at the same quality.
Is cast polyurethane the same as TPU?
No. TPU is a thermoplastic that is injection molded, extruded or printed and can be remelted. Cast polyurethane is a two-part thermoset that cures in the mold. Both span similar hardness ranges, but they are processed differently and their datasheets are not interchangeable.
Can cast urethane be used for food-contact or medical parts?
Only with resins specifically certified for that use and with validation by the customer; most casting resins are intended for prototypes and pre-series parts. For regulated parts, use the production material, for example LSR or a certified thermoplastic.
Related resources
- Silicone MoldingRTV, LSR and soft-tool silicone workflows.
- Bridge ProductionPlanning the step from prototype to volume.
- Standard SLA ResinSmooth printed master patterns.
- PolyJet Rigid OpaqueFine-detail masters and visual models.
- Liquid Silicone Rubber (LSR)Production elastomer for seals and soft parts.
- TPU 95AThermoplastic elastomer alternative.
- Injection MoldingWhen volumes justify tooling.
- Quality Control & InspectionFirst article and inspection scope.
Related materials
Can't find what you need? Contact our team for expert assistance with your manufacturing project.