A356 (EN AC-42100, AlSi7Mg0.3) is an aluminum casting alloy with about 7% silicon and 0.3% magnesium. The silicon gives fluidity and resistance to hot cracking; the magnesium makes it heat-treatable. In the T6 condition (solution-treated, quenched and artificially aged) it combines good strength with better ductility than most aluminum casting alloys, helped by its low iron content (≤ 0.20%).
Choose it for complex aluminum parts in quantities that justify a pattern or mold: housings, brackets, pump and valve bodies, wheels and structural castings that must be pressure-tight, weldable or heat-treated. A356 is a gravity and low-pressure casting alloy; high-pressure die casting normally uses A380-type alloys instead.
Mechanical and physical properties
| Property | Typical value (T6) | Notes |
|---|---|---|
| Tensile strength (Rm) | ≈ 250–280 MPa | Permanent-mold castings at the upper end. ASTM B26 minimum for sand-cast A356.0-T6: 234 MPa. |
| Yield strength (Rp0.2) | ≈ 180–210 MPa | ASTM B26 minimum for sand-cast T6: 165 MPa. |
| Elongation at break | ≈ 3–10% | Sand castings at the lower end, permanent-mold castings higher; porosity reduces it sharply. |
| Hardness | ≈ 70–90 HB | Softer than 6061-T6 (95 HB). |
| Elastic modulus | ≈ 72 GPa | Slightly stiffer than wrought aluminum alloys. |
| Fatigue strength | ≈ 60–90 MPa | Rotating beam, 5 × 10⁸ cycles; very sensitive to porosity and surface condition. |
| Density | 2.68 g/cm³ | About one-third of steel or cast iron. |
| Thermal conductivity | ≈ 150 W/m·K | T6 condition; good for housings that must shed heat. |
| Thermal expansion | ≈ 21.5 µm/m·K | 20–100 °C; lower than wrought alloys because of the silicon. |
| Electrical conductivity | ≈ 39% IACS | T6 condition. |
| Melting range | ≈ 555–615 °C | Plan feeding of thick sections with the foundry. |
Typical values for A356-T6 test bars. Properties in a real casting depend on the process, section thickness, soundness and heat treatment, and are usually lower in thick or porous sections. Use the minimums of the governing standard (e.g. ASTM B26/B108, EN 1706) and, for critical parts, test data from separately cast bars or specimens cut from the casting.
Casting A356: routes and design rules
A356 is poured by gravity into sand or permanent (metal) molds, filled by low-pressure casting, or cast into investment shells. The route sets tooling cost, surface, accuracy and properties:
| Route | Tooling | Typical use | Notes |
|---|---|---|---|
| Sand casting | Low: pattern and core boxes | Prototypes, large parts, low volumes | Roughest surface, widest tolerances, lowest properties. |
| Permanent mold (gravity die) | Medium: steel or iron mold | Medium volumes, repeat parts | Finer surface, tighter dimensions and higher properties than sand. |
| Low-pressure casting | Medium to high | Wheels, structural parts | Controlled, calm filling for sound castings. |
| Investment casting | Medium: wax-pattern tooling | Small, detailed parts | Fine detail and surface; limited part size. |
- Uniform walls: Uretyco's casting guidance links porosity to thick sections and sudden wall transitions. Keep walls as even as possible, blend changes gradually and core out heavy bosses.
- Draft, radii and parting line: plan them together with gating; generous fillets improve metal flow and reduce hot tears.
- Machining allowance and datums: critical sealing surfaces, bearing bores and datum features are usually machined after casting, so show machining allowances and a datum scheme on the drawing.
- Heat treatment: state the temper (usually T6). Quenching can distort thin or asymmetric castings, so machine critical features after heat treatment.
- Pressure tightness: state the test pressure and medium; where the specification allows, porosity can be sealed by vacuum impregnation.
- First article: Uretyco's quality guidance lists first-article or sample approval for castings before a full run.
Machining and welding
In the T6 condition A356 machines well and leaves a good finish; the hard silicon particles wear tools faster than wrought alloys, so production machining uses carbide or PCD tooling. The alloy is weldable by TIG with 4043 filler, which is also used for casting repairs where the specification allows them; welding locally removes the T6 strength unless the casting is heat-treated again.
Tolerances and surface
Cast-surface tolerances depend on the route, part size and supplier, and are confirmed in the quote and the order. Specify them with a casting tolerance standard such as ISO 8062-3 and put tight tolerances only on machined features. Machined features can be toleranced like CNC parts, where Uretyco's default for unspecified tolerances is ISO 2768-mK. Sand castings are rougher than permanent-mold or investment castings; call out Ra only on machined faces that need it.
Finishing options
The high silicon content limits decorative anodizing, so conversion coatings and paint systems are the usual choice. Plan finishing together with machining and masking.
| Finish | What it adds | Notes for A356 |
|---|---|---|
| Shot or bead blast | Uniform matte surface | Removes scale and sand residue; common base finish. |
| Chromate conversion | Corrosion protection, paint base | Negligible build-up; keeps the surface conductive. |
| Powder coat or wet paint | Color, protection | Over a conversion coat; gas in porosity can cause pinholes, so castings are often pre-baked. |
| Anodize | Protection | Grey, uneven appearance due to silicon; protective rather than decorative. |
| Machined faces | Sealing and fits | Mask during coating; state Ra and flatness only where needed. |
Heat treatment can move thin walls, so machine critical features after T6 and apply conversion coating or paint last. Mask machined sealing faces and threads, and state whether dimensions apply before or after coating.
- Surface Finish GuideCoatings, paint and drawing callouts.
- Surface FinishingProcess overview, masking and quality notes.
Cost and lead-time drivers
Castings carry a one-time tooling cost (pattern, core boxes or a permanent mold) and a per-part cost that falls with quantity. The main levers:
- Tooling and quantity: sand patterns suit low volumes; permanent molds cost more but pay back on repeat orders. Quote realistic annual quantities.
- Cores and complexity: internal passages need cores, which add tooling, labor and scrap risk.
- Secondary operations: heat treatment, impregnation, machining and coating are separate steps, each with its own lead time.
- Quality scope: first-article approval, inspection reports and material certificates are opt-in; documented inspection can extend the lead time. Special tests such as pressure testing must be part of the order scope.
A356-T6 vs. common alternatives
| Material | Typical process | Strength (Rm) | Elongation | Heat-treatable | Best for |
|---|---|---|---|---|---|
| A356-T6 | Sand, permanent mold, low pressure | ≈ 250–280 MPa | ≈ 3–10% | Yes | Pressure-tight, weldable, structural castings |
| A380 | High-pressure die casting | ≈ 320 MPa (as cast) | ≈ 3% | Not usually | Thin-walled, high-volume parts |
| A357-T6 | Sand, permanent mold, investment | Higher than A356 | Similar or lower | Yes | Higher-strength, often aerospace castings |
| 6061-T6 (machined) | CNC from plate or bar | ≈ 310 MPa | 12–17% | Yes | Low quantities, no tooling |
Below the quantity that pays for a pattern or mold, machining the part from 6061-T6 is usually faster and avoids casting risk; Uretyco's die-casting guidance likewise points to CNC machining when volumes are low or tolerances leave little room for casting variation. For thin-walled, high-volume parts, high-pressure die casting in A380-type alloys costs less per part but is not usually heat-treated and is less ductile.
When not to choose A356
Very low quantities where machining avoids tooling: use 6061-T6. Thin-walled, high-volume parts: consider high-pressure die casting in an A380-type alloy. Decorative anodized surfaces. Continuous service above about 150 °C, where the T6 temper over-ages. Fatigue-critical parts without a defined soundness requirement and inspection plan.
Typical applications
- Pump, gearbox and transmission housings.
- Pressure-tight valve bodies and manifolds.
- Automotive wheels, cylinder heads and suspension parts.
- Marine fittings and outdoor structural castings.
- Brackets, frames and machine components.
- Aerospace and defense castings (often in A357).
Specifying A356 on Uretyco
- 1Specify alloy, temper and route
A356-T6 or EN AC-42100 T6, and whether sand or permanent mold is required or left open.
- 2Upload STEP of the cast part plus a drawing
Show machined surfaces with allowance, datums, the cast tolerance standard, pressure-test requirements and finish.
- 3Plan first article and documents at quote time
First-article approval, inspection reports and material certificates are opt-in; asking after production usually means re-inspection.
FAQ
What is the difference between A356 and 356?
Both have the same silicon and magnesium ranges, but A356 limits iron to 0.20% (356: 0.6%) and copper to 0.20%, which gives better ductility and fatigue strength. Specify A356 when elongation or fatigue matters.
What is A356 called in European standards?
EN AC-42100 (EN AC-AlSi7Mg0.3) under EN 1706. The related EN AC-42000 (AlSi7Mg) corresponds to 356 with its higher iron limit, so confirm substitutions for certified parts.
Can A356 be high-pressure die cast?
It is not a typical high-pressure die-casting alloy: it tends to stick to steel dies, and conventional die castings trap gas that blisters during T6 heat treatment. Uretyco's die-casting page covers high-pressure zinc and aluminum alloys; A356 belongs to gravity, low-pressure and some special high-integrity processes.
Is A356 pressure-tight?
It is one of the preferred alloys for pressure-tight castings, but tightness depends on design and foundry practice. State the test pressure and medium on the drawing; where acceptable, porosity can be sealed by vacuum impregnation before finishing.
Related resources
- Molding & Casting OverviewShared files, design themes and tolerance notes.
- Die CastingHigh-pressure casting for zinc and aluminum.
- Aluminum 6061-T6Machined alternative for low quantities.
- CNC MachiningFor machined features on castings.
- Quality Control & InspectionFirst article, reports and certificates.
- Technical Drawings & TolerancesWhat belongs on the 2D drawing.
- Choosing the Right ProcessCasting vs. machining vs. sheet metal.
- Lead Time AnatomyWhere order time goes.
Related materials
Can't find what you need? Contact our team for expert assistance with your manufacturing project.