Aluminum 3003-H14 (EN AW-3003, AlMn1Cu) is a non-heat-treatable alloy with about 1.2% manganese. The manganese makes it about 20% stronger than commercially pure aluminum while keeping its formability, weldability and corrosion resistance. H14 means strain-hardened to a half-hard condition.
Choose it for formed sheet parts that carry little load: decorative and architectural panels, kitchen and food-service equipment, HVAC ducting, covers and trim. It folds, hems and seams easily with modest springback. When a bent part must also carry load or survive seawater, 5052-H32 is the stronger choice.
Mechanical and physical properties
| Property | Typical value | Notes |
|---|---|---|
| Tensile strength (Rm) | 150 MPa | Specification range ≈ 140–180 MPa (ASTM B209). |
| Yield strength (Rp0.2) | 145 MPa | Specification minimum ≈ 115 MPa. Yield is close to tensile strength in H14. |
| Elongation at break | 8–16% | ≈ 8% in 1.6 mm sheet; higher in thicker gauges and in softer tempers. |
| Hardness | 40 HB | Soft surface; dents and scratches easily. |
| Elastic modulus | 69 GPa | About one-third of steel; large flat panels need flanges or beads. |
| Fatigue strength | ≈ 62 MPa | Rotating beam, 5 × 10⁸ cycles; about half of 5052-H32. |
| Density | 2.73 g/cm³ | About one-third of steel. |
| Thermal conductivity | 159 W/m·K | Good for heat-exchanger fins and cookware. |
| Thermal expansion | 23.2 µm/m·K | 20–100 °C; about twice steel. |
| Electrical conductivity | ≈ 41% IACS | Bare or conversion-coated surfaces stay conductive. |
Typical room-temperature handbook values for 3003-H14 sheet; actual values vary with thickness and mill. For structural calculations, use the minimums of the governing standard (e.g. ASTM B209, EN 485-2) or your material certificate.
Laser cutting and bending 3003-H14
3003 cuts and bends easily, so most problems come from its softness rather than from cracking. It is not in the K-factor table of Uretyco's sheet-metal guide; the guide notes that a generic K-factor of 0.44 is close for aluminum, and its 5052 values (inside radius equal to the thickness, K ≈ 0.40–0.43) are a sensible starting point. Rules to apply:
- Bend radius: thin 3003-H14 can often be bent tighter than the thickness, but design at an inside radius equal to the thickness unless the supplier confirms a smaller one. Refine the K-factor with supplier feedback.
- Holes and edges: hole diameter at least the sheet thickness, at least 2× thickness from an edge and 3× thickness from the bend tangent line.
- Bends and reliefs: keep 6× thickness plus the bend radii between neighbouring bends, and add reliefs at least 1× thickness wide and 1.5× thickness deep where a bend meets an edge.
- Stiffness: the low yield strength means large flat panels dent and oil-can. Add return flanges, hems or stiffening beads rather than thickening the sheet.
- Cosmetic faces: the soft surface marks during cutting, bending and handling. Name the visible face, and ask whether protective film can stay on during fabrication.
Tolerances and surface
Uretyco's sheet-metal guide gives these achievable values: ±0.10 mm on laser-cut edge lengths and hole diameters (holes for fits are drilled), bend angles ±1° as standard and ±0.5° on request, hole positions after bending ±0.5 mm by default, and 1–2 mm of possible warp on parts longer than 300 mm. Thin, soft 3003 panels are especially prone to that warp, so control flatness only where it matters. Laser-cut edges are slightly oxidized; ask for deburring if the part is handled. Final values are confirmed in the quote and the order.
Finishing options
3003 is mostly used bare, brushed, painted or powder coated. It anodizes for protection, but its manganese content gives a greyer, less even tone than 6061 or anodizing-quality sheet such as 5005.
| Finish | What it adds | Notes for 3003-H14 |
|---|---|---|
| Mill finish, deburred | Lowest cost | Forms a protective oxide; rolling and handling marks remain visible. |
| Brushed | Uniform linear grain | Popular for kitchen and decorative panels; specify grain direction. |
| Anodize Type II | Corrosion protection | Protective rather than decorative; dyed colors look less even than on 6061. |
| Chromate conversion | Corrosion protection, paint base | Negligible build-up; keeps the surface conductive. |
| Powder coat or wet paint | Color, tough coating | ≈ 60–100 µm powder over a conversion coat; the usual choice for colored panels. |
Bend and hem before anodizing or powder coating, and state whether dimensions apply before or after finishing. For anodized decorative panels, ask about an anodizing-quality alloy such as 5005 instead of 3003.
- Surface Finish GuideAnodize types, coatings and drawing callouts.
- Surface FinishingProcess overview, masking and quality notes.
Cost and lead-time drivers
As with any sheet part, the work matters more than the alloy. Uretyco's sheet-metal guidance names these drivers:
- Cutting: material thickness, sheet size, cut length, pierce count, tiny holes and nesting efficiency.
- Forming: number and complexity of bends, hems and tool changes; bending adds setup, tooling, sequence planning and inspection compared with a flat cut.
- Finishing and cosmetics: brushing, coating color, masking and cosmetic acceptance criteria can drive lead time more than fabrication.
- Availability: Uretyco's sheet-metal page lists 5052, 5754 and 6061 as typical aluminum sheet. If 3003 is not readily available, allowing an approved equivalent in the order notes can speed up supplier matching.
3003-H14 vs. common sheet alternatives
| Material | Strength | Formability | Corrosion | Weldability | Relative cost |
|---|---|---|---|---|---|
| 3003-H14 | Baseline (Rm ≈ 150 MPa) | Excellent | Good | Excellent | Baseline |
| 5052-H32 | Higher (Rm ≈ 230 MPa) | Good; inside radius = thickness | Very good, incl. marine | Very good | Similar or higher |
| 1050A-H14 | Lower (Rm ≈ 105–145 MPa) | Excellent | Very good | Excellent | Similar |
| Galvanized steel DX51D | Higher (Rm ≈ 270–500 MPa) | Good | Good while the zinc is intact; cut edges exposed | Good, with zinc-fume precautions | Lower |
| Stainless 304 | Much higher (Rm ≈ 515 MPa) | Good; more springback | Excellent | Excellent | Higher |
For most enclosures and brackets, 5052-H32 costs little more and is about half again as strong, so 3003 makes sense mainly where forming, appearance or thermal conductivity lead. Stainless 304 replaces it in food-service equipment that sees heavy cleaning, impact or abrasion.
When not to choose 3003-H14
Load-bearing brackets, frames or mounts: the strength is low; use 5052-H32 or steel. Seawater immersion or splash zones: use 5052. Precision machined parts: 3003 is gummy and soft. Decorative dyed anodize: use an anodizing-quality alloy. Parts that must stay dent-free in use, such as unprotected kick panels.
Typical applications
- Decorative architectural panels, cladding trim and signage.
- Kitchen, cookware and food-service equipment panels.
- HVAC ducts, hoods and ventilation parts.
- Heat-exchanger fins and housings.
- Light-duty covers, enclosures and trim.
- Storage containers and lightweight tanks.
Specifying 3003-H14 on Uretyco
- 1Select 3003-H14, thickness and finish
Use a standard thickness; note acceptable equivalents such as 5052 or 5754 if strength and corrosion allow.
- 2Upload DXF, STEP and drawing
A 1:1 DXF for flat parts; for bent parts a STEP of the formed part plus a PDF drawing with bend direction, inside radius, visible face and grain direction.
- 3Define cosmetic acceptance
State visible faces, brushing direction, coating color and acceptable marks before ordering; certificates and inspection reports are opt-in at quote time.
FAQ
3003 or 5052 for a bent enclosure?
Usually 5052-H32: it bends at an inside radius equal to the thickness, is about half again as strong and handles marine environments better. Choose 3003 when panels are heavily formed or hemmed, mainly decorative, or when its higher thermal conductivity helps.
What is 3003 called in European standards?
EN AW-3003, chemical designation EN AW-AlMn1Cu (former material number 3.0517); H14 means the same in EN 515. Confirm any substitution, for example with 3103 or 3105 sheet, before ordering certified parts.
Can 3003 be welded or brazed?
Yes. It welds very well by TIG or MIG, typically with 4043 filler, and it is a common alloy for brazed assemblies such as heat exchangers. Welding removes the H14 work hardening locally, so the weld zone drops to annealed strength.
Is 3003 suitable for food equipment?
It is a long-established alloy for cookware and food-service panels. Suitability for a specific food-contact part depends on the alloy specification, surface finish and use conditions, since acidic or salty foods attack bare aluminum. State the requirement in the order notes; for heavy cleaning or abrasion, stainless 304 is the safer choice.
Related resources
- Sheet Metal Design GuideBend radii, K-factors, hole rules and DXF hygiene.
- Sheet Metal & Laser CuttingProcess overview, files, tolerances and cost drivers.
- DXF Files for Laser CuttingHow to prepare a clean flat pattern.
- Aluminum 5052-H32Stronger sheet alloy for bent and marine parts.
- Galvanized SteelLower-cost, zinc-protected steel sheet.
- Stainless Steel 304Hygienic, abrasion-resistant sheet.
- Designing for Lower CostStandard thicknesses, fewer bends, simpler finishes.
- Technical Drawings & TolerancesWhat belongs on the 2D drawing.
Related materials
Can't find what you need? Contact our team for expert assistance with your manufacturing project.