Aluminum 7075-T6 (EN AW-7075) is a heat-treatable Al-Zn-Mg-Cu alloy in the T6 temper: solution heat-treated and artificially aged. It is one of the strongest common aluminum alloys, with roughly 1.7–1.8× the tensile strength of 6061-T6 at almost the same density, which puts it in the range of many carbon steels at about one-third of their density.
Choose it for highly loaded, weight-critical machined parts: aerospace fittings, drone and robot structures, performance sporting components and stiff tooling plates. The price for that strength is lower corrosion resistance, no practical fusion weldability, less ductility and higher stock cost. If 6061-T6 is strong enough, it remains the better default.
Mechanical and physical properties
| Property | Typical value | Notes |
|---|---|---|
| Tensile strength (Rm) | 572 MPa | Specification minimums ≈ 525–540 MPa for plate up to ≈ 60 mm; lower in thicker sections. |
| Yield strength (Rp0.2) | 503 MPa | Specification minimums ≈ 440–470 MPa, by product form and thickness. |
| Elongation at break | ≈ 11% | Specification minimums ≈ 5–8%; noticeably less ductile than 6061-T6. |
| Hardness | 150 HB | ≈ 175 HV. |
| Elastic modulus | 71.7 GPa | Only ≈ 4% stiffer than 6061; the extra strength adds no stiffness. |
| Fatigue strength | ≈ 159 MPa | Rotating beam, 5 × 10⁸ cycles. Notch-sensitive; generous radii matter. |
| Density | 2.81 g/cm³ | ≈ 36% of steel. |
| Thermal conductivity | 130 W/m·K | Lower than 6061 (167 W/m·K). |
| Thermal expansion | ≈ 23.4 µm/m·K | Similar to 6061, about twice steel. |
| Electrical conductivity | ≈ 33% IACS | Anodized surfaces are insulating. |
| Service temperature | Up to ≈ 100–120 °C | Long exposure above ≈ 120 °C over-ages the T6 temper and permanently reduces strength. |
Typical room-temperature handbook values for wrought 7075-T6/T651; actual values vary with product form, thickness and mill. For structural calculations, use the minimums of the governing standard (e.g. ASTM B209/B221, EN 485-2/EN 755-2) or your material certificate.
Machining 7075-T6
7075-T6 is one of the most pleasant aluminum alloys to machine. It is harder and less gummy than 6061, so chips break more cleanly, burrs are smaller and fine finishes are easier to reach with sharp carbide tools at high speeds. Plate is usually supplied as T651 (stress-relieved by stretching), bar as T6 or T6511. Watch for:
- Residual stress and movement: heavy material removal from thick plate can still release stress and bow thin floors or long walls. Balance stock removal between faces and call out flatness only where it matters.
- Thin walls: the CNC Design Guide treats walls under 0.8 mm in aluminum as risky, with pocket depth up to about 4× the narrowest opening. The higher strength resists permanent bending, but stiffness and chatter behave as in 6061.
- Internal corners and notches: keep internal radii at least one-third of the pocket depth (sharp corners need EDM). 7075 is more notch-sensitive than 6061, so radius loaded corners and avoid sharp undercuts in stressed areas.
- Threads: use standard sizes (M2–M10), 1.5–3× the diameter deep. 7075 threads are stronger than 6061 threads but still wear under repeated assembly; use threaded inserts there.
- Stock sizes: Uretyco's aluminum comparison notes that 7075 stock thicknesses are more limited than 6061. Check availability before designing around an unusual plate thickness.
Tolerances and surface finish
Uretyco treats unspecified tolerances as ISO 2768-mK, with a default as-machined surface of around Ra 1.6–3.2 µm and light deburring. Tighter tolerances, finer Ra values and fits need a 2D drawing and belong on functional features only. As with 6061, thermal expansion is about twice that of steel, so inspect tight tolerances on large parts at 20 °C. Final values are confirmed in the quote and the order.
Finishing options
Unlike 6061, 7075 should almost never be left bare outside a dry indoor environment. Its zinc and copper content make it more prone to pitting, exfoliation and stress corrosion, so plan a protective finish together with the design.
| Finish | What it adds | Notes for 7075-T6 |
|---|---|---|
| As-machined | Lowest cost | Acceptable only for dry indoor parts and prototypes; marks and tarnishes with handling. |
| Bead blast | Uniform matte look | Hides light tool marks; follow with anodize or conversion coating for protection. |
| Anodize Type II | Corrosion protection, color | 5–25 µm. Anodizes well, but clear can look slightly yellowish and dyed colors are less even than on 6061. Electrically insulating. |
| Hard anodize Type III | Wear resistance, best protection | Typically 25 µm and up; dark grey to bronze. Common on 7075; lowers fatigue strength, so radius sharp edges. |
| Chromate conversion | Corrosion protection, paint base | Negligible build-up and stays conductive; for outdoor 7075 parts usually combined with paint. |
| Powder coat or paint | Color, barrier protection | ≈ 60–100 µm (powder) over a conversion coat; mask threads and mating faces. |
About half of an anodic layer grows outward and half penetrates the metal, so a 25 µm hard-anodize layer shrinks a bore, or grows a pin, by roughly 25 µm on diameter. State whether dimensions apply before or after finishing, and mask threads, bearing bores and electrical contact faces.
- Surface Finish GuideAnodize types, coatings and drawing callouts.
- Surface FinishingProcess overview, masking and quality notes.
Cost and lead-time drivers
As a rule of thumb, material is typically 10–30% of a CNC quote, machine time 35–55% and finishing 0–25%. Uretyco's aluminum comparison puts 7075 at about 1.6–1.9× the cost of 6061, so on bulky parts the alloy premium is noticeable; on small, feature-heavy parts machine time still dominates. The main levers:
- Stock: standard plate and bar sizes keep lead time down; stock material is usually faster than a special order. Certified material or unusual sizes add time.
- Setups: a part machined in two setups costs roughly half of one that needs four. Deep pockets and small cutters add machine time.
- Finishing: Type II anodize typically adds 10–25% and Type III 25–50%, plus batch time. On 7075 a finish is usually required, so budget for it from the first quote.
- Documents: material certificates, inspection reports and CMM measurements are opt-in and can extend the lead time. Request them at quote time.
7075-T6 vs. common alternatives
| Material | Strength | Machinability | Corrosion | Weldability | Relative cost |
|---|---|---|---|---|---|
| 7075-T6 | Baseline (Rm ≈ 570 MPa) | Good; cleaner chips than 6061 | Fair; needs protection | Not recommended | Baseline (≈ 1.6–1.9× 6061) |
| 6061-T6 | ≈ 55% (Rm ≈ 310 MPa) | Good | Good | Good; weld zone softens | Lower |
| 2024-T351 | ≈ 80% (Rm ≈ 470 MPa); better fatigue | Good | Fair; needs protection | Not recommended | Slightly lower (≈ 1.4–1.7× 6061) |
| 7075-T7351 | ≈ 88% (Rm ≈ 505 MPa) | Good | Better; resists stress corrosion | Not recommended | Similar to slightly higher |
| Titanium Ti-6Al-4V | ≈ 1.7× (Rm ≈ 950 MPa); 58% heavier | Difficult | Excellent | Possible with inert-gas shielding | Much higher |
| Steel 4140 (pre-hardened) | ≈ 1.6–1.8× (Rm ≈ 900–1050 MPa); ≈ 2.8× heavier | Fair | Poor; needs coating | Needs preheat | Cheaper stock, slower machining |
Per unit weight, 7075-T6 outperforms pre-hardened 4140 and comes close to Ti-6Al-4V, but its elastic modulus is only about one-third of steel's, so stiffness-limited parts need larger sections in any aluminum alloy. Where stress corrosion is a risk, for example sustained tension through the plate thickness, the overaged T7351 temper gives up roughly 10–15% of the strength for much better resistance.
When not to choose 7075-T6
Welded assemblies: 7075 is prone to hot cracking, so use 6061 or bolted and riveted joints. Marine, wet or salt-exposed parts without a sealed finish: use 6061 or 5052, or protect 7075 thoroughly. Continuous service above about 120 °C. Bent sheet or formed parts: 7075-T6 cracks in tight bends. Decorative dyed anodize where color matching matters: 6061 anodizes more evenly. Sustained tension through the thickness of thick plate: consider T7351.
Typical applications
- Aerospace and UAV fittings, brackets and frames.
- Robot arms, end effectors and highly loaded linkages.
- Motorsport, cycling and other performance sporting components.
- Stiff tooling plates, jigs and fixture components under high clamping loads.
- Mold inserts for prototype and low-volume injection molding.
- Hard-anodized wear parts such as gears, cams and slides under moderate loads.
Specifying 7075-T6 on Uretyco
- 1Select 7075-T6 and a protective finish
Hard anodize or Type II anodize for most parts; chromate conversion plus paint where conductivity or a paint base is needed. State T7351 if stress corrosion matters.
- 2Upload STEP plus a 2D drawing
Needed for anything tighter than ISO 2768-mK, threads, Ra, masking or GD&T. Mark whether dimensions apply before or after anodizing.
- 3Request documents at quote time
Material certificates and inspection reports are opt-in; ask for them in the quote, not after shipment.
FAQ
What is the difference between 7075-T6, T651 and T7351?
T651 is T6 plate stress-relieved by stretching (T6511 for extruded bar): same properties, less machining distortion. T7351 is overaged: about 10–15% lower strength, but much better resistance to stress corrosion cracking and exfoliation. State the temper on the drawing if it matters.
What is 7075 called in European standards?
EN AW-7075, chemical designation EN AW-AlZn5.5MgCu (former DIN material number 3.4365). It is widely stocked as plate and bar in Europe and Türkiye, though in fewer sizes than 6082 or 6061.
Can 7075-T6 be welded?
Not by conventional TIG or MIG for structural joints: it is prone to hot cracking and the heat-affected zone loses much of its strength. Design bolted, pinned or riveted joints, or use 6061 if welding is unavoidable.
Is 7075-T6 as strong as steel?
Its tensile strength (≈ 570 MPa) exceeds mild steel such as 1018 (≈ 440 MPa cold-drawn) and approaches some medium-carbon steels, at about one-third of the density. But its elastic modulus (≈ 72 GPa) is also about one-third of steel's, so a part of the same size deflects about three times as much. For wear surfaces or high-cycle fatigue, hardened steel is still the better choice.
Related resources
- Aluminum 6061-T6The default aluminum: weldable and anodizes evenly.
- Aluminum 6061 vs 7075 vs 2024When to step up from 6061 to 7075 or 2024.
- Titanium Grade 5Higher strength, heat and corrosion resistance.
- Alloy Steel 4140Hardenable steel for wear and stiffness.
- Aluminum 5052-H32Bent sheet parts and marine service.
- CNC Design GuideTolerances, walls, threads and setups.
- CNC MachiningProcess overview, files and cost drivers.
- Technical Drawings & TolerancesWhat belongs on the 2D drawing.
- Lead Time AnatomyWhere order time goes.
Related materials
Can't find what you need? Contact our team for expert assistance with your manufacturing project.