17-4 PH (UNS S17400, AISI 630, EN 1.4542 / X5CrNiCuNb16-4) is a martensitic stainless steel with about 17% chromium, 4% nickel and 4% copper. It is supplied solution-annealed (Condition A) and strengthened by a single aging treatment at about 480–620 °C that precipitates copper-rich particles. Aging takes place in air with little distortion, so parts can be machined close to size first and hardened afterward.
Choose 17-4 PH when a part needs much more strength than 304 or 316L while keeping stainless corrosion behavior: roughly twice the tensile strength and 3.5–6 times the yield strength of annealed 304. Shafts, valve stems, fasteners, fittings and mechanism parts are typical. Its corrosion resistance is broadly comparable to 304 in many environments but well below 316L in chlorides, and choosing the right aging condition matters as much as choosing the alloy.
Mechanical and physical properties
| Condition | Aging temperature | Rm (min.) | Rp0.2 (min.) | Elongation (min.) | Hardness |
|---|---|---|---|---|---|
| H900 | 482 °C | 1310 MPa | 1170 MPa | 10% | ≥ 40 HRC |
| H1025 | 552 °C | 1070 MPa | 1000 MPa | 12% | ≥ 35 HRC |
| H1075 | 579 °C | 1000 MPa | 860 MPa | 13% | ≥ 32 HRC |
| H1150 | 621 °C | 930 MPa | 725 MPa | 16% | ≥ 28 HRC |
| Condition A | None (solution-annealed) | Not specified | Not specified | Not specified | ≤ 38 HRC; for machining, not for service |
| Property | Typical value | Notes |
|---|---|---|
| Density | 7.78 g/cm³ | Similar to other stainless steels. |
| Elastic modulus | ≈ 197 GPa | Similar to other steels. |
| Thermal conductivity | ≈ 18 W/m·K | Slightly higher than 304. |
| Thermal expansion | ≈ 11 µm/m·K | Lower than austenitic 304/316 (≈ 17), closer to carbon steel. |
| Magnetic | Yes | Martensitic structure; unsuitable where parts must be non-magnetic. |
| Service temperature | Up to ≈ 315 °C | Longer exposure above this reduces toughness. |
| Size change on aging | Contraction of ≈ 0.05% (H900) to ≈ 0.1% (H1150) | Small and predictable; compensate on tight features or finish after aging. |
The condition table lists ASTM A564 minimums for bar; typical values are higher. Toughness, ductility and stress-corrosion resistance improve from H900 to H1150 while strength falls. For design, use the governing specification (ASTM A564, AMS 5643 or EN 10088-3) or your material certificate.
Machining and heat-treatment sequence
The usual route is simple: machine in Condition A, age to the required condition, then passivate. Watch for:
- Machinability: Condition A machines roughly like 304, tough on tools and prone to work hardening. Use rigid setups, sharp tools and steady feeds. Uretyco's stainless selection guide recommends this route, aging to H1025 or H1075 after machining where the shape allows.
- Aging contraction: parts shrink slightly when aged (≈ 0.05% for H900, up to ≈ 0.1% for H1150). On tight fits, compensate in the machining dimensions or leave stock and finish after aging.
- Condition A is not a service condition: it has lower toughness and stress-corrosion resistance than aged material. Always state the final condition on the drawing.
- Walls, pockets and threads: the CNC Design Guide's stainless values apply (1.2 mm minimum walls, pockets up to 3:1); keep threads to standard sizes (M2–M10), 1.5–3× the diameter deep.
- Welding: possible, but full properties require solution treatment and re-aging afterward, so plan welded assemblies around the heat treatment.
Tolerances and surface finish
Uretyco treats unspecified tolerances as ISO 2768-mK with an as-machined surface around Ra 1.6–3.2 µm and light deburring. State on the drawing whether dimensions apply before or after aging and passivation. Heat treatment adds lead time; final values are confirmed in the quote and the order.
Passivation and finishes
Machined stainless picks up free iron from tools and handling, and aging leaves a light heat tint. Passivation per ASTM A967 after final machining and aging restores the passive layer; specify it explicitly for any part in corrosive service.
| Finish | What it adds | Notes for 17-4 PH |
|---|---|---|
| As-machined | Lowest cost | Heat tint from aging remains unless removed. |
| Passivation (ASTM A967) | Restores corrosion resistance | Recommended after machining and aging; no dimensional change. |
| Bead blast | Uniform matte look | Removes heat tint; follow with passivation. |
| Electropolish | Smooth, clean, bright surface | Removes a small amount of material; allow for it on fits. |
| Mirror polish | Optical or sealing surfaces | Below Ra 0.4 µm; typically +50–150%. |
Any process that heats the part above its aging temperature afterward, such as some coatings or brazing, changes the condition. Coordinate high-temperature finishes with the heat treatment.
Cost and lead-time drivers
Uretyco's stainless selection guide puts 17-4 PH at about 1.6× the cost of 304. Beyond the stock price, the main levers are:
- Machine time: Condition A cuts like 304, slower than carbon steel and with more tool wear; deep pockets and small cutters add up quickly.
- Heat treatment: aging is a separate furnace step that adds lead time. H900 and H1150 are equally simple, so choose the condition on performance, not price.
- Stock: standard bar sizes are widely available; certified or special sizes add time, while stock material is usually faster.
- Documents: material certificates and inspection reports are opt-in and can extend the lead time; request them at quote time.
17-4 PH vs. common alternatives
| Material | Strength (Rm) | Corrosion | Machinability | Magnetic | Relative cost |
|---|---|---|---|---|---|
| Stainless 17-4 PH | ≈ 930–1310 MPa (H1150–H900) | Good; similar to 304 in many media | Fair (Condition A) | Yes | ≈ 1.6× 304 |
| Stainless 304 | ≈ 515 MPa | Very good | Poor to fair; work-hardens | No (slightly when cold-worked) | Baseline |
| Stainless 316L | ≈ 485 MPa | Excellent, including chlorides | Poor to fair | No | ≈ 1.4× 304 |
| Alloy steel 4140, pre-hardened | ≈ 900–1050 MPa | Poor; needs a coating | Fair | Yes | Lower |
| Titanium Grade 5 | ≈ 950 MPa | Excellent | Difficult | No | Much higher |
15-5 PH, a close relative with better toughness across the grain, is a common substitute in aerospace drawings; confirm availability before specifying it.
When not to choose 17-4 PH
Seawater immersion, chloride crevices or splash zones: 316L or duplex grades resist pitting better. H900 parts under impact or in stress-corrosion-prone service: choose H1025–H1150 instead. Service above about 315 °C. Non-magnetic requirements. Simple parts that need only moderate strength: 304 is cheaper and needs no heat treatment.
Typical applications
- Pump shafts, valve stems and valve trim.
- High-strength fasteners, pins and bushings.
- Aerospace fittings and actuator parts.
- Gears, couplings and mechanism parts in wet environments.
- Mold components and fixtures that need corrosion resistance.
- Oil and gas components; sour-service rules (NACE MR0175 / ISO 15156) require specific double-aged conditions.
Specifying 17-4 PH on Uretyco
- 1Select 17-4 PH and the final condition
H900 for maximum strength, H1025–H1075 for balanced properties, H1150 for toughness and stress-corrosion resistance.
- 2Upload STEP plus a 2D drawing
State whether dimensions apply after aging, and add passivation, thread and finish callouts.
- 3Request documents at quote time
Certificates and hardness or inspection reports must be planned before production.
FAQ
Which condition should I specify?
H900 gives the highest strength but the lowest toughness and stress-corrosion resistance. H1025 or H1075 is a good general-purpose balance, and H1150 suits impact, sour service or parts that must not crack. Never specify Condition A for service.
What is 17-4 PH called in European standards?
1.4542, X5CrNiCuNb16-4 (EN 10088), also known as AISI 630. EN 10088 names heat-treatment conditions by minimum tensile strength (for example +P1070) rather than H-numbers, so state the required condition explicitly.
Is 17-4 PH magnetic?
Yes, in all conditions, because its structure is martensitic. Use 316L where a non-magnetic stainless part is required.
Is 17-4 PH available as a 3D-printed metal?
It is one of the most common stainless steels for laser powder-bed fusion (DMLS/SLM), although printed parts need their own heat treatment and do not exactly match wrought properties. Uretyco's 3D printing guidance lists stainless among the metal options and reserves metal printing for geometry that machining cannot make practically.
Related resources
- Stainless 304 vs 316L vs 17-4 PHChoosing between the three grades.
- Stainless Steel 304The default austenitic stainless.
- Stainless Steel 316LFor chlorides and marine exposure.
- Alloy Steel 4140Lower-cost strength where corrosion is not an issue.
- Inconel 718When temperatures exceed the range of 17-4 PH.
- CNC Design GuideTolerances, walls, threads and setups.
- Surface Finish GuidePassivation, electropolishing and drawing callouts.
- Technical Drawings & TolerancesWhat belongs on the 2D drawing.
Related materials
Can't find what you need? Contact our team for expert assistance with your manufacturing project.