Brass C360 (UNS C36000, free-cutting brass) is a copper-zinc alloy with about 61.5% copper, 35% zinc and ≈ 3% lead. The lead forms fine particles at which chips break into small fragments, which is why C360 is the reference (100%) on the copper-alloy machinability scale. Its closest European equivalents are CW603N (CuZn36Pb3) and the very common CW614N (CuZn39Pb3).
Choose it for turned and milled parts made in volume: fittings, connectors, valve parts, precision screws and decorative hardware. It machines faster than any other common metal, holds tolerances well, needs no protective finish in normal environments, and is non-magnetic and non-sparking. It is not a high-strength material, and its lead content rules it out for drinking water and many food-contact applications.
Mechanical and physical properties
| Property | Typical value | Notes |
|---|---|---|
| Tensile strength (Rm) | ≈ 400 MPa | Half-hard (H02) rod; ≈ 340 MPa soft-annealed, up to ≈ 470 MPa in small diameters. |
| Yield strength (Rp0.2) | ≈ 310 MPa | Half-hard rod; soft-annealed ≈ 125–140 MPa. |
| Elongation at break | ≈ 25% | Half-hard; ≈ 50% soft-annealed. |
| Hardness | ≈ 78 HRB | Half-hard rod; soft-annealed material is considerably softer. |
| Elastic modulus | ≈ 97 GPa | About half of steel; parts deflect more than steel parts of the same size. |
| Density | 8.5 g/cm³ | ≈ 3× aluminum, slightly heavier than steel. |
| Thermal conductivity | ≈ 115 W/m·K | About twice carbon steel. |
| Thermal expansion | ≈ 20.5 µm/m·K | Between steel and aluminum. |
| Electrical conductivity | ≈ 26% IACS | Good for connectors; pure copper is ≈ 100%. |
| Machinability rating | 100% | Reference value for copper alloys; C260 ≈ 30%, C110 ≈ 20%. |
| Magnetic behavior | Non-magnetic | Suitable near sensors and magnets. |
Typical room-temperature values for C36000 rod; strength depends on temper (soft-annealed to hard) and bar diameter. For calculations, use the minimums of the governing standard (e.g. ASTM B16, EN 12164) or your material certificate.
Machining C360 brass
C360 is the easiest metal to machine: short broken chips, low cutting forces, very high speeds, long tool life and a bright finish straight off the tool. It is the classic material for bar-fed lathes and Swiss-type turning. Watch for:
- Thin walls: the CNC Design Guide sets 0.6 mm as the practical minimum for brass C360 and allows pocket depths up to about 5× the opening, the most generous values among the metals it lists.
- Grabbing: brass can pull a drill or cutter into the work, so zero or slightly negative rake tools are used. Avoid features that rely on heavy interrupted cuts in thin sections.
- Burrs: burrs are small and easy to remove, so tight edge-break requirements add little cost.
- Threads: use standard sizes (M2–M10), 1.5–3× the diameter deep. Brass threads cut cleanly, including fine pitches, but wear under repeated assembly; use steel inserts or design for limited cycles.
- Stress and cold work: heavily cold-worked or stressed brass can crack in ammonia-containing environments (stress corrosion, known as season cracking). Avoid high residual stress in press fits for such service.
Tolerances and surface finish
Uretyco treats unspecified tolerances as ISO 2768-mK, with a default as-machined surface of around Ra 1.6–3.2 µm and light deburring. Brass naturally machines to a bright, smooth surface, but if Ra matters, state it on a 2D drawing together with tighter tolerances and fits. Final values are confirmed in the quote and the order.
Finishing options
Brass needs no protective finish: it resists corrosion in air, fresh water and most indoor environments. Bare brass darkens over time, so finishes are mainly about appearance, contact performance or preventing tarnish.
| Finish | What it adds | Notes for C360 |
|---|---|---|
| As-machined | Lowest cost | Bright, clean surface that tarnishes gradually. The right choice for most technical parts. |
| Polish | Bright decorative surface | Usually combined with lacquer to keep the shine. |
| Clear lacquer | Tarnish protection | Thin transparent coating; can wear on frequently handled surfaces. |
| Nickel plating | Silver look, wear and tarnish resistance | Common on visible hardware and as an underlayer for chrome or gold. |
| Tin, silver or gold plating | Solderability and contact performance | For electrical connectors and terminals; specify the thickness on contact areas. |
| Bead blast | Uniform matte look | Hides tool marks on cosmetic parts. |
Nickel, tin and silver build up on every surface, so a 5 µm layer grows a pin by about 10 µm on diameter. State whether dimensions apply before or after plating, and mark areas that must stay bare, such as threads or press fits.
- Surface Finish GuidePolish, lacquer, plating and drawing callouts.
- Surface FinishingProcess overview, masking and quality notes.
Cost and lead-time drivers
As a rule of thumb, material is typically 10–30% of a CNC quote, machine time 35–55% and finishing 0–25%. Brass stock costs more per kilogram than aluminum or steel because of its copper content, but very short cycle times can make C360 the cheapest choice for small turned parts in volume. The main levers:
- Stock form: round, hex and square rod suit bar-fed turning; designing the part around a standard bar size reduces waste and machining.
- Quantity: setup cost is spread over more parts, and brass rewards larger batches because cycle times are short.
- Setups: a part machined in two setups costs roughly half of one that needs four; keep features accessible from as few directions as possible.
- Documents: material certificates and inspection reports are opt-in and can extend the lead time. If lead-free material is required, say so at quote time.
C360 vs. common alternatives
| Material | Machinability | Strength | Corrosion | Lead | Typical use |
|---|---|---|---|---|---|
| C360 / CW614N | 100% (reference) | Rm ≈ 400 MPa | Good in air and fresh water | ≈ 3% | Turned parts, fittings, connectors |
| Lead-free brass (CW724R / C69300) | Good, below C360 | Similar to higher | Good | Lead-free | Drinking water, regulated products |
| Brass C260 (CuZn30) | ≈ 30% | Similar (Rm ≈ 300 MPa annealed, higher cold-worked) | Good | Lead-free | Cold-formed, drawn and decorative parts |
| Bronze C932 | ≈ 70% | Rm ≈ 240 MPa | Very good | Contains ≈ 7% lead | Bushings and plain bearings |
| Aluminum 6061-T6 | Good | Rm ≈ 310 MPa | Good | None | Light housings and brackets |
| Copper C110 | ≈ 20% | Rm ≈ 220–360 MPa | Good | None | Electrical conductors |
Choose C360 when machining time dominates and lead is acceptable. For drinking water or lead-restricted products, use a lead-free brass and accept slower machining; for bushings and sliding parts, bearing bronze C932; for electrical conductors, copper C110; and for light, non-decorative structural parts, 6061-T6.
When not to choose C360
Drinking-water parts and many food-contact or consumer products: C360 contains ≈ 3% lead; use an approved low-lead or lead-free brass. Ammonia-containing atmospheres combined with stress: risk of season cracking. Aggressive or stagnant water that causes dezincification: use a dezincification-resistant (DZR) brass. Highly loaded structural parts: strength and stiffness are modest; consider steel or 7075-T6. Welded assemblies: leaded brass is not suitable for fusion welding; soldering works well.
Typical applications
- Pneumatic and hydraulic fittings, adapters and valve components (not for drinking water).
- Electrical connectors, terminals, contacts and threaded inserts.
- Precision turned parts: screws, nuts, spacers, pins and shafts for instruments.
- Pinions, bushings and parts for clocks, meters and measuring instruments.
- Decorative and architectural hardware: knobs, handles and trim.
- Non-magnetic parts near sensors and magnets.
Specifying C360 on Uretyco
- 1Select C360 (or state that CW614N is acceptable)
If the part must be lead-free, do not choose C360; say so and name the required standard or approval.
- 2Upload STEP plus a 2D drawing
Needed for anything tighter than ISO 2768-mK, threads, Ra, plating areas or GD&T.
- 3Choose the finish and documents
As-machined, polish and lacquer, or plating with a thickness; request material certificates at quote time if the lead content must be documented.
FAQ
What is C360 called in European standards?
The closest match is CW603N (CuZn36Pb3). In practice, CW614N (CuZn39Pb3) is the most widely stocked free-cutting brass in Europe and Türkiye; it contains slightly more zinc and machines almost as well. Confirm substitutions on certified parts.
Can C360 be used for drinking water?
No. Leaded free-cutting brass is not suitable for parts in contact with drinking water. Use a brass approved for drinking water, typically a low-lead or lead-free grade such as CW511L or CW724R, and check the approval required in your market.
Does C360 need a finish?
Not for corrosion protection in normal environments. Bare brass tarnishes slowly, which many technical parts can tolerate. Choose polish and lacquer or nickel plating for visible parts, and tin, silver or gold for electrical contacts.
C360 or C260?
C360 machines about three times better (rating 100 vs ≈ 30) and is the choice for turned and milled parts. Lead-free C260 cartridge brass is far more ductile, so choose it for parts that are cold-formed, bent, drawn or stamped, or where lead is not allowed and machining volumes are low.
Related resources
- Brass C260Lead-free brass for cold-formed parts.
- Bronze C932Leaded bearing bronze for bushings.
- Copper C110Maximum electrical conductivity.
- Aluminum 6061-T6Lighter structural alternative.
- Stainless Steel 304Corrosion-resistant steel for stronger parts.
- CNC Design GuideTolerances, walls, threads and setups.
- CNC MachiningProcess overview, files and cost drivers.
- Technical Drawings & TolerancesWhat belongs on the 2D drawing.
- Quality Control & InspectionInspection scope, reports and certificates.
Related materials
Can't find what you need? Contact our team for expert assistance with your manufacturing project.