C260 (UNS C26000), also known as cartridge brass, is a 70/30 copper-zinc alloy: about 70% copper, 30% zinc and practically no lead (0.07% maximum). As a single-phase alpha brass it is very ductile: in the annealed condition it withstands deep drawing, spinning, tight bending and stamping that would crack free-cutting brass. It polishes to a bright gold finish and is widely available as sheet, strip, rod and tube.
Choose C260 when the part is formed from sheet or strip, when lead must be kept low, or when a cold-worked temper is needed for stiffness or spring. For complex parts machined from bar, free-cutting C360 is usually cheaper because it cuts roughly three times faster; C260 earns its place only when its formability or low lead content is actually used.
Mechanical and physical properties
| Property | Typical value | Notes |
|---|---|---|
| Tensile strength (Rm) | ≈ 300–370 MPa (annealed) | Rises with cold work: ≈ 350–490 MPa quarter- to half-hard, ≈ 480–560 MPa hard. |
| Yield strength (Rp0.2) | ≈ 75–160 MPa (annealed) | ≈ 170–360 MPa quarter- to half-hard; above ≈ 430 MPa hard. |
| Elongation at break | ≈ 45–65% (annealed) | Falls steeply with cold work; hard tempers are below ≈ 10%. |
| Hardness | ≈ 55–90 HV (annealed) | ≈ 95–155 HV quarter- to half-hard. Specify the temper rather than a hardness value where possible. |
| Elastic modulus | ≈ 110 GPa | About 55% of steel. |
| Density | 8.53 g/cm³ | About 3.2× aluminum 6061. |
| Thermal conductivity | ≈ 120 W/m·K | About 70% of aluminum 6061-T6. |
| Electrical conductivity | ≈ 28% IACS | Adequate for terminals and lamp contacts; use copper C110 where conductivity matters. |
| Thermal expansion | ≈ 20 µm/m·K | Between steel (≈ 12) and aluminum (≈ 24). |
| Melting range | ≈ 915–955 °C | Readily brazed and soldered. |
| Machinability rating | 30 (C360 = 100) | Long, stringy chips; see the machining notes below. |
Values depend strongly on temper (annealed, quarter-hard, half-hard, hard) and product form. For design, use the minimums of the governing standard (e.g. ASTM B36 or EN 1652 for sheet and strip) or your material certificate, and state the temper on the drawing.
Machining C260
Without the lead of free-cutting brass, C260 forms long, continuous chips and smears on dull tools. It is still far easier to machine than steel or stainless, but cycle times are longer than for C360 and chip control needs attention. Watch for:
- Chip control: use sharp, positive-rake tools with chip-breaking geometry; long chips wrap around turned parts and mark finished surfaces.
- Temper: annealed stock is gummy; half-hard rod or plate cuts more cleanly and holds size better.
- Thin walls: the CNC Design Guide gives 0.6 mm and a 5:1 pocket ratio for free-cutting C360. Treat these as the limit for C260, not a target, because the gummier alloy deflects and burrs more.
- Burrs: Uretyco's default is light deburring; specify an edge break where burrs at hole exits and slot edges matter.
- Threads: standard sizes (M2–M10), 1.5–3× the diameter deep. Brass threads suit occasional assembly; use threaded inserts for frequent assembly cycles.
Sheet metal and forming
Formability is the reason to choose C260. Order the temper that matches the operation: annealed or quarter-hard for deep drawing, spinning and tight bends; half-hard for flat or lightly bent parts that need stiffness or spring. Harder tempers need larger bend radii and spring back more.
- Flat profiles: copper alloys reflect laser light strongly and are normally cut on fiber lasers. Send a clean 1:1 DXF in millimeters.
- The sheet metal guide's feature rules apply: holes at least as large as the thickness, at least 2× thickness from edges and 3× thickness from bend tangent lines, and bend reliefs at least one thickness wide and 1.5× thickness deep.
- Brass is not in the guide's K-factor table; model with your CAD default and let the supplier confirm the flat pattern where dimensions across bends are critical.
- Bend angles are ±1° as standard (±0.5° on request), and hole positions after bending ±0.5 mm by default.
- Season cracking: cold-worked 70/30 brass can crack under residual stress in ammonia-bearing atmospheres. For heavily formed parts in such service, specify a stress-relief anneal (around 250–300 °C) after forming.
Tolerances and surface finish
For machined parts, Uretyco treats unspecified tolerances as ISO 2768-mK, with an as-machined surface around Ra 1.6–3.2 µm and light deburring. Laser-cut edge lengths are typically held to ±0.10 mm. Tighter tolerances, cosmetic faces and finer Ra values need a 2D drawing; final values are confirmed in the quote and the order.
Finishing options
Bare brass darkens from bright gold to brown with handling and humidity. For decorative parts, decide how the surface should age before ordering.
| Finish | What it adds | Notes for C260 |
|---|---|---|
| As-machined or mill finish | Lowest cost | Tarnishes; fingerprints mark polished faces. |
| Brushed | Uniform satin look | Hides handling marks; state the grain direction on visible faces. |
| Polished | Bright, reflective surface | Mirror polish (below Ra 0.4 µm) is a large cost adder, typically +50–150%. |
| Clear lacquer | Keeps the polished color | Thin organic coat; wears through on high-touch surfaces. |
| Nickel plating | Durable silver-colored finish, corrosion protection | Bright or satin; decorative chrome is plated over nickel. Mask threads and fits. |
On formed and polished parts, mark the visible face and grain direction on the drawing so cutting, bending and handling protect that side.
Cost and lead-time drivers
Copper alloys cost more per kilogram than aluminum and are three times as dense, so material can take a larger share of a brass quote than the 10–30% typical for CNC parts. The main levers:
- Process: cut and bent parts are priced on cut length, pierces, bends and material; machined parts on machine time, which is longer for C260 than for C360.
- Temper and form: standard sheet, strip and rod are widely stocked; unusual thicknesses or tempers can mean a special order, while stock material is usually faster.
- Finishing: polishing and plating are often the largest added cost on decorative parts, plus batch time at the finisher.
- Documents: material certificates and inspection reports are opt-in and can extend the lead time; request them at quote time.
C260 vs. common alternatives
| Material | Strength (Rm) | Machinability | Formability | Notes |
|---|---|---|---|---|
| Brass C260 | ≈ 300–560 MPa by temper | Fair (30) | Excellent | Low lead (≤ 0.07%); bright gold color. |
| Brass C360 | ≈ 340–400 MPa | Excellent (100) | Limited; cracks in tight bends | ≈ 3% lead; fastest-machining brass. |
| Copper C110 | ≈ 220 MPa (annealed) | Poor (20) | Excellent | ≈ 100% IACS conductivity; gummy to machine. |
| Aluminum 5052-H32 | ≈ 230 MPa | Fair; gummy | Very good | One-third of the weight; good seawater resistance. |
| Stainless 304 | ≈ 515 MPa | Poor to fair | Good; springs back more | No tarnish; excellent corrosion resistance. |
In European standards the closest match is CuZn30 (CW505L). CuZn37 (CW508L) is the more widely stocked general-purpose sheet brass in Europe and is also low in lead, but it is less ductile in deep drawing; confirm any substitution before ordering certified parts.
When not to choose C260
Complex parts machined from bar with no forming step and no lead restriction: C360 machines faster. Wetted drinking-water parts: 70/30 brass is not dezincification-resistant. Cold-worked parts in ammonia-bearing environments without stress relief. Seawater immersion: choose a bronze or stainless grade. High strength, wear or elevated temperature: consider bronze, steel or stainless. Conductors where electrical losses matter: use copper C110.
Typical applications
- Deep-drawn cups, shells and housings.
- Cartridge cases, eyelets, rivets and snap fasteners.
- Decorative trim, nameplates, kick plates and architectural hardware.
- Lamp fittings, sockets and reflectors.
- Musical instrument components.
- Springs and clips in half-hard or hard tempers.
Specifying C260 on Uretyco
- 1Select C260 and state the temper
Annealed, quarter-hard, half-hard or hard; note CuZn30 (CW505L) or another equivalent if acceptable.
- 2Upload the right files
STEP for machined or bent parts, a clean DXF for flat profiles, and a 2D drawing for tolerances, bends, cosmetic faces and grain direction.
- 3Define finish and documents at quote time
Polish, lacquer or plating, masking areas, and any certificates or inspection reports.
FAQ
What is C260 called in European standards?
CuZn30, material number CW505L (formerly 2.0265 or Ms70). Composition limits differ slightly from UNS C26000, so confirm the equivalent when certified material is required.
Should I use C260 or C360 for a machined part?
Usually C360: it cuts roughly three times faster and breaks into short chips. Choose C260 when the same part is also formed, when lead content is restricted, or when you need its higher ductility.
Can C260 be used in drinking-water systems?
Its lead content is very low, but 70/30 brass can dezincify in some waters, leaving porous, weak copper. For wetted drinking-water components, use a dezincification-resistant (DZR) brass or an alloy approved under the applicable national rules.
How do I keep brass parts bright?
Polish and clear-lacquer them for indoor decorative use, or nickel-plate parts that are handled often. Unprotected brass darkens over months, which is acceptable or even wanted on some architectural parts.
Related resources
- Brass C360Free-cutting brass for machined parts.
- Copper C110When electrical conductivity comes first.
- Aluminum 5052-H32Light, formable sheet with good corrosion resistance.
- Stainless Steel 304When corrosion resistance comes first.
- Sheet Metal & Laser GuideBend rules, K-factor and DXF hygiene.
- Sheet Metal & Laser CuttingProcess overview, files and cost drivers.
- CNC Design GuideTolerances, walls, threads and setups.
- Surface Finish GuidePolish, lacquer, plating and drawing callouts.
- Technical Drawings & TolerancesWhat belongs on the 2D drawing.
Related materials
Can't find what you need? Contact our team for expert assistance with your manufacturing project.