Uretyco
Make it now
Copper C110 (ETP)

Copper C110 (ETP)

Metals
CopperC110ElectricalConductive

Copper C110 (ETP, Cu-ETP/CW004A) reference: typical properties by temper, CNC machining notes, plating and finishing for contacts and bus bars, cost drivers, and comparison with C101, C145, CuCrZr, brass C360 and aluminum.

Copper C110 (UNS C11000, electrolytic tough pitch, EN Cu-ETP / CW004A) is at least 99.90% copper with a small, deliberate oxygen content of about 0.02–0.04%. Apart from silver, it has the highest electrical and thermal conductivity of any common engineering metal: at least 100% IACS and roughly 390 W/m·K.

Choose it for parts whose job is to carry current or heat: bus bars, terminals, grounding parts, contacts, heat spreaders and induction coils. Its weaknesses are low strength, poor machinability (soft, gummy and burr-prone) and fast tarnishing. Its oxygen content also rules it out for hydrogen atmospheres and some brazing processes, where oxygen-free copper is required. Besides CNC milling and turning, C110 can be ordered through Uretyco for sheet metal; 3D printing of copper is covered in the FAQ.

Mechanical and physical properties

PropertyTypical valueNotes
Electrical conductivity≥ 100% IACS≈ 58 MS/m; the reference for conductor sizing. Cold work lowers it only slightly.
Thermal conductivity≈ 390 W/m·KAbout 2.3× aluminum 6061.
Tensile strength (Rm)≈ 220–360 MPaRises with cold work: ≈ 220 MPa annealed (R220), ≈ 290 MPa half-hard (R290), ≥ 360 MPa hard (R360).
Yield strength (Rp0.2)≈ 70–320 MPa≈ 70 MPa annealed; ≈ 250–320 MPa half-hard to hard.
Elongation at break≈ 45% (annealed)Drops sharply with cold work.
Hardness≈ 40–120 HV≈ 40–65 HV annealed; ≥ 110 HV hard.
Elastic modulus≈ 115–117 GPaAbout 1.7× aluminum, a little over half of steel.
Density≈ 8.9 g/cm³≈ 3.3× aluminum.
Thermal expansion≈ 17 µm/m·KSimilar to stainless 304; about 1.4× steel.
Machinability rating≈ 20%Relative to brass C360 = 100%; tellurium copper C145 ≈ 85%.
SofteningAbove ≈ 200 °CHard tempers lose strength at elevated temperature; brazing fully anneals the part.
Typical values, not design allowables

Typical room-temperature values; mechanical properties depend strongly on temper (annealed to hard) and product form. For calculations, use the minimums of the governing standard (e.g. ASTM B152/B187, EN 13601/EN 1652) or your material certificate.

Machining C110 copper

Pure copper is one of the harder common metals to machine well. It is soft and ductile, so it smears onto tools, forms long stringy chips and leaves heavy burrs; it also deforms easily under clamping. Very sharp, polished tools with a high positive rake, high cutting speeds and plenty of coolant give the best results. Watch for:

  • Burrs: expect burrs at every edge and hole exit; specify edge breaks, and remember that manual deburring adds cost. Uretyco's default is light deburring.
  • Clamping and thin sections: soft copper dents and springs; avoid thin, unsupported walls and mark cosmetic or contact faces that must not carry clamp marks. The CNC Design Guide gives no copper-specific minimum wall, so treat its 0.8–1.2 mm figures for other metals as a lower bound and check thin features in the DFM findings.
  • Internal corners: copper loads small cutters heavily; keep internal radii generous, at least one-third of the pocket depth as for other metals.
  • Threads: tapped threads in soft copper strip easily and can gall. For threaded electrical joints, use through-bolts, threaded inserts or a free-machining copper such as C145, which threads cleanly.
  • Temper: half-hard (H02) bar machines more cleanly than soft annealed stock; specify the temper if strength or bendability matters.

Tolerances and surface finish

Uretyco treats unspecified tolerances as ISO 2768-mK, with a default as-machined surface of around Ra 1.6–3.2 µm and light deburring. Contact faces, the flatness of bus-bar joints and plated areas should be defined on a 2D drawing, together with any tighter tolerances. Because copper expands about 1.4× as much as steel, check large parts at a stable temperature. Final values are confirmed in the quote and the order.

Finishing options

Bare copper tarnishes quickly and shows fingerprints. On electrical parts, plating is chosen for contact resistance, solderability and corrosion protection rather than looks.

FinishWhat it addsNotes for C110
As-machinedLowest cost, best bare conductivityOxidizes and tarnishes; clean contact faces before assembly.
Tin platingSolderability, stable contacts, corrosion protectionThe usual bus-bar and terminal finish; also used where copper meets aluminum conductors.
Silver platingLow contact resistance, high-current jointsFor switchgear and high-current contacts.
Nickel platingWear and corrosion barrierHarder surface; also an underlayer for gold.
Gold over nickelReliable low-force signal contactsThin layers on contact areas only.
Polish and clear lacquerDecorative finishFor visible parts; lacquer insulates, so mask electrical contact faces.
Mask the contact faces

Specify plating thickness and where it is required, mark faces that must stay bare or unpainted for electrical contact, and state whether dimensions apply before or after plating. Uretyco's Surface Finish Guide lists polish, lacquer and nickel or silver plating for copper.

Cost and lead-time drivers

As a rule of thumb, material is typically 10–30% of a CNC quote, machine time 35–55% and finishing 0–25%. Copper stock is expensive per kilogram, and bulky bus bars can push the material share to the top of that range; slow, careful machining and deburring add time on top. The main levers:

  • Make flat parts from sheet or flat bar: simple bus bars and terminals are often cheaper as cut and bent sheet than as fully machined parts; compare both routes.
  • Reduce material removal: start from standard flat or round bar sizes close to the finished shape.
  • Burrs and cosmetics: edge-break and cosmetic requirements on copper mean manual work; apply them only where needed.
  • Plating and documents: plating adds a finishing step and batch time. Material certificates and inspection reports are opt-in and can extend the lead time; request them at quote time.

C110 vs. common alternatives

MaterialConductivity (IACS)MachinabilityStrengthTypical use
C110 (Cu-ETP)≥ 100%≈ 20%Rm ≈ 220–360 MPaBus bars, terminals, heat spreaders
C101/C102 (oxygen-free, Cu-OFE / Cu-OF)≥ 100%≈ 20%SimilarHydrogen brazing, vacuum and high-reliability parts
C145 (tellurium copper)≈ 93%≈ 85%SimilarMachined contacts, connectors, EDM electrodes
CuCrZr (C18150)≈ 75–80%FairRm ≈ 400 MPa or more (aged)Welding electrodes, parts that run hot
Brass C360≈ 26%100%Rm ≈ 400 MPaConnectors where machining cost dominates
Aluminum 6061-T6≈ 43%GoodRm ≈ 310 MPaLight bus bars and heat sinks

For equal conductance, a 6061-T6 conductor needs about 2.3× the cross-section of copper and is still lighter; dedicated conductor aluminum such as 1350 or 6101 does better. When a copper part has many machined features, C145 is the usual compromise.

When not to choose C110

Common mismatches

Hydrogen brazing, hydrogen atmospheres or high-vacuum parts: the oxygen in ETP copper causes hydrogen embrittlement; use oxygen-free C101 or C102. Heavily machined parts with many threads and fine features: consider C145, or brass if conductivity allows. Structural or highly loaded parts: copper is weak and creeps; consider CuCrZr, brass, bronze or steel. Parts that run continuously hot under load: hard tempers soften above ≈ 200 °C. Weight-sensitive conductors and heat sinks: consider aluminum.

Typical applications

  • Bus bars, current-carrying links and bus-bar connectors.
  • Terminals, cable lugs and grounding parts.
  • Switchgear and relay contacts, usually plated.
  • Heat spreaders, cold plates and heat-sink bases for electronics.
  • Induction coils and RF or EMI shielding components.
  • EDM electrodes.

Specifying C110 on Uretyco

  1. 1
    Select C110 and its temper

    Choose half-hard for most machined parts; specify oxygen-free C101/C102 if the part will be hydrogen-brazed or used in vacuum.

  2. 2
    Upload STEP plus a 2D drawing

    Mark contact faces, plating areas and thickness, joint flatness and any tolerances tighter than ISO 2768-mK.

  3. 3
    Request documents at quote time

    Material certificates and inspection reports are opt-in; if conductivity must be verified, say so before production.

FAQ

What is the difference between C110 and C101?

Both conduct at ≈ 100% IACS. C110 (Cu-ETP) contains a little oxygen, which makes it cheaper but causes embrittlement when it is heated in hydrogen, for example during hydrogen brazing. C101 (Cu-OFE) and C102 (Cu-OF) are oxygen-free, cost more and are used for brazed, welded, vacuum and high-reliability parts.

What is C110 called in European standards?

Cu-ETP, material number CW004A (EN 13601 for rod and bar, EN 1652 for plate and sheet). It is the standard electrical copper in Europe and Türkiye and is widely stocked as flat bar for bus bars.

Does C110 need plating?

Not for structural reasons, but almost always for electrical joints that must stay reliable. Tin is the default for bus bars and terminals, silver for high-current contacts, and nickel or gold for wear and signal contacts. Bare copper joints work if the contact faces are cleaned and protected.

Copper or aluminum for a bus bar?

Copper carries more current in a given space and makes compact, reliable joints. Aluminum is lighter and cheaper per ampere but needs a larger cross-section, careful joint design and protection against galvanic corrosion where it meets copper. For compact assemblies choose copper; for long, weight-sensitive runs, aluminum.

Can copper be 3D printed?

Yes, by laser powder bed fusion (DMLS or SLM), but it is a specialized route. Pure copper reflects most of the infrared laser light used by standard metal printers and conducts the heat away quickly, so it is printed with green or blue lasers, which it absorbs far better, or with high-power infrared lasers. As printed, its conductivity is lower than that of wrought C110; an annealing heat treatment brings dense parts close to it. CuCrZr is easier to print and stronger, but reaches its typical ≈ 70–80% IACS only after aging. Printing suits induction coils, heat exchangers and cold plates with internal cooling channels that cannot be machined. Feasibility, alloy and heat treatment are confirmed in the quote.

Related materials

Was this page helpful?

Can't find what you need? Contact our team for expert assistance with your manufacturing project.

Contact our team