A2 (AISI A2, UNS T30102, EN 1.2363 / X100CrMoV5) is a cold-work tool steel with about 1% carbon, 5% chromium and 1% molybdenum. It hardens fully in still air from about 925–980 °C, so it distorts far less in heat treatment than oil- or water-hardening grades, and it balances wear resistance and toughness better than most steels in its class.
Choose A2 for tooling and wear parts that must hold an edge or a precise shape at around 60 HRC: punches, dies, forming tools, gauges and wear plates. It is bought annealed, machined soft, hardened, and then finish-ground or EDM-cut on the critical features. If a part only needs to be strong and stiff, a pre-hardened alloy steel such as 4140 is cheaper and faster.
Mechanical and physical properties
| Property | Typical value | Notes |
|---|---|---|
| Hardness, as supplied | ≈ 200–250 HB | Annealed condition, used for machining. |
| Hardness, hardened and tempered | 57–62 HRC | Set by the tempering temperature; give a range on the drawing, e.g. 58–60 HRC. |
| Tensile strength | Not usually specified | Hardness is the acceptance criterion for tool steels. |
| Toughness | Medium-high for its class | Tougher than D2, less tough than shock-resisting S7. |
| Wear resistance | Good | Between O1 and D2. |
| Elastic modulus | ≈ 200 GPa | Similar to other steels. |
| Density | 7.86 g/cm³ | Similar to other steels. |
| Thermal conductivity | ≈ 25 W/m·K | About half of plain carbon steel. |
| Thermal expansion | ≈ 11 µm/m·K | Close to plain carbon steel. |
| Size change in hardening | Small | Far less than oil- or water-hardening steels, but not zero; leave grinding stock on precision features. |
Typical handbook values; hardness, toughness and size change depend on section size, heat-treatment cycle and steel supplier. For critical tooling, follow the steel supplier's heat-treatment data and specify the hardness range and its test location on the drawing.
Machining and heat-treatment sequence
A2 parts are made in two stages: machine the steel soft, then harden it and finish only what must be precise. A typical route:
- Rough-machine annealed stock, leaving finishing allowance on precision faces, bores and profiles. A2 cuts more slowly than mild steel or 4140 and wears tools faster, but it is predictable.
- For heavily machined or asymmetric parts, a stress-relief anneal after roughing reduces movement during hardening.
- Harden and temper, usually in vacuum or a protective atmosphere to avoid decarburization; otherwise leave stock to grind away the soft skin. Double tempering is common practice.
- Finish critical features by grinding, hard milling or wire EDM. Wire EDM leaves a thin recast layer; on highly stressed cutting edges, specify skim passes or a stress-relieving temper after EDM.
- Machine threads and non-critical holes before hardening; tapping at 60 HRC is not practical.
Design for heat treatment as well as for machining: generous internal radii and gradual section changes reduce cracking and distortion, while sharp internal corners and holes close to edges are classic crack starters. The CNC Design Guide's steel values (1.0 mm minimum wall, pockets up to 3:1) are a floor for soft machining; hardened tooling usually needs much more material for support.
Tolerances and surface finish
Uretyco treats unspecified tolerances as ISO 2768-mK with an as-machined surface around Ra 1.6–3.2 µm. On hardened tooling, every tighter tolerance implies grinding, hard milling or EDM after heat treatment, so mark which features are critical and state that their dimensions apply after hardening. Heat treatment adds lead time; final values are confirmed in the quote and the order.
Finishes and coatings
With 5% chromium, A2 resists staining better than carbon steel, but it is not stainless: unprotected parts rust in humid storage.
| Finish | What it adds | Notes for A2 |
|---|---|---|
| As-ground or as-machined, oiled | Lowest cost | Standard for internal tooling; keep oiled in storage. |
| Black oxide | Mild corrosion resistance, dark finish | Negligible build-up; needs oil to protect. |
| Nitriding | Harder, more wear-resistant surface | Process temperature exceeds low tempering temperatures; plan it together with the heat treatment. |
| PVD coating (TiN, TiCN, CrN or similar) | Low friction, longer edge life | Applied at roughly 400–500 °C, so A2 must be tempered above the coating temperature, typically leaving ≈ 57–58 HRC. |
| Mirror polish | Smooth forming and molding surfaces | Below Ra 0.4 µm; a large cost adder, typically +50–150%. |
If the part will be nitrided or coated, say so before heat treatment. The tempering temperature has to suit the later process; otherwise the coating cycle softens the steel.
Cost and lead-time drivers
A2 parts cost more than the stock price suggests, because hardening and post-hardening finishing are separate operations with their own queues. As a rule of thumb, material is typically 10–30% of a CNC quote; on hardened tooling, work after heat treatment can be the largest item. The main levers:
- Heat treatment: an extra process step that adds lead time; vacuum hardening costs more than open-atmosphere processes but reduces grinding.
- Post-hardening finishing: grinding and wire EDM are slower than soft machining, so limit them to the features that need them.
- Stock: standard flat and round sizes are widely stocked; stock material is usually faster than a special order.
- Documents: inspection reports (including hardness results) and material certificates are opt-in and can extend the lead time; request them at quote time.
A2 vs. other tool and alloy steels
| Material | Typical working hardness | Wear resistance | Toughness | Heat-treat distortion | Machinability (soft) |
|---|---|---|---|---|---|
| A2 (1.2363) | 57–62 HRC | Good | Good | Very low (air-hardening) | Fair |
| D2 (1.2379) | 58–62 HRC | Very high | Lower | Very low | Poor to fair |
| O1 (1.2510) | 57–62 HRC | Moderate | Moderate | Low to moderate (oil-hardening) | Good |
| S7 | 54–58 HRC | Moderate | Very high (shock-resisting) | Low | Fair |
| 4140, pre-hardened | 28–32 HRC | Low | High | None (supplied hardened) | Fair |
Choose D2 when abrasive wear dominates and impact is low, S7 when edges chip or tools see shock, and O1 for simple, lower-cost tooling where some distortion is acceptable. When in doubt, A2 is the safe middle ground.
When not to choose A2
Corrosive or wet environments: use a stainless grade such as 17-4 PH. Service above the tempering temperature, or hot work: A2 softens, so use a hot-work steel such as H13. Heavy shock or impact: S7 is tougher. Severe abrasive wear: D2, powder-metallurgy steels or carbide last longer. Fixtures and structural parts that need only moderate strength: 4140 or 1018 cost less and need no hardening.
Typical applications
- Blanking and piercing punches and dies.
- Forming, bending and trimming tools.
- Gauges, setting masters and inspection fixtures.
- Wear plates, guides and shear blades.
- Mold inserts where wear resistance matters.
- Industrial knives and slitter blades.
Specifying A2 on Uretyco
- 1Select A2 and state the hardness range
For example 58–60 HRC, with the test location; note 1.2363 if acceptable.
- 2Upload STEP plus a 2D drawing
Mark features finished after hardening, grinding allowances, edge conditions and any coating.
- 3Request documents at quote time
Hardness results, inspection reports and certificates must be planned before production.
FAQ
A2 or D2?
D2 contains more carbide and lasts longer against abrasive wear, but it is less tough and harder to machine and grind. A2 is the better choice when edges chip or parts see moderate impact.
What is A2 called in European standards?
1.2363, X100CrMoV5 (EN ISO 4957). It is directly comparable to AISI A2, but confirm equivalence with the supplier for certified tooling.
Can I order A2 parts already hardened?
Yes. Specify the hardness range and which features are finished after hardening. Heat treatment adds a process step and lead time, so include it in the quote rather than adding it later.
Does A2 rust?
Yes. Its chromium content slows staining compared with carbon steel, but it is not stainless. Keep parts oiled, or specify black oxide, nitriding or a PVD coating.
Related resources
- Alloy Steel 4140Pre-hardened steel for fixtures and shafts.
- Carbon Steel 1018Low-cost steel for parts that need no hardening.
- Stainless Steel 17-4 PHHardenable and corrosion-resistant.
- CNC Design GuideTolerances, walls, threads and setups.
- CNC MachiningProcess overview, files and cost drivers.
- Technical Drawings & TolerancesWhat belongs on the 2D drawing.
- Quality Control & InspectionInspection scope, reports and certificates.
- Lead Time AnatomyWhere order time goes.
Related materials
Can't find what you need? Contact our team for expert assistance with your manufacturing project.