PLA (polylactic acid) is a thermoplastic made from plant sugars such as corn starch or sugarcane. It prints at low temperatures, barely warps and needs no heated chamber, so FDM parts in PLA come out stiff, dimensionally faithful and with crisp detail. It is the cheapest and most forgiving FDM material and is available in a very wide range of colors.
Choose PLA for visual prototypes, form and fit checks, presentation models and light-duty indoor fixtures. Its limits are clear: it softens at around 55–60 °C, is brittle under impact, creeps under sustained load and degrades outdoors. For anything warm, loaded, flexed or outdoors, step up to PETG, ASA or a powder-bed nylon.
Mechanical and physical properties
| Property | Typical value | Notes |
|---|---|---|
| Tensile strength | ≈ 45–60 MPa | Printed in the layer plane (XY); across layers (Z) it can be far lower. |
| Elongation at break | ≈ 2–6% | Brittle: snaps rather than bends. |
| Tensile modulus | ≈ 2.3–3.5 GPa | Stiffer than PETG, ABS or ASA. |
| Density | 1.24 g/cm³ | Solid material; printed parts weigh less, depending on infill. |
| Glass transition (Tg) | ≈ 55–65 °C | Above Tg the part softens and deforms. |
| Heat deflection temperature | ≈ 50–55 °C | At 0.45 MPa, unannealed. |
| Max service temperature | ≈ 50 °C | Lower under sustained load. |
| Impact resistance | Low | Thin features and snap-fits crack. |
| UV and outdoor resistance | Poor to moderate | Fades and embrittles over months outdoors. |
| Compostability | Industrial only | Breaks down in industrial composting, not in soil, water or home compost within a useful time. |
Typical filament datasheet values. Printed parts depend strongly on orientation, layer height, wall count, infill and printing temperature, and vary between brands. Validate load-bearing parts with real printed samples in the expected environment.
Printing PLA with FDM
FDM builds parts from extruded beads, layer by layer. The process, more than the polymer, decides what you get from a PLA part:
- Orientation: parts are weakest between layers. Orient them so the main loads and any clips run along the layers, and say so in the order notes if orientation matters.
- Infill and walls: FDM parts are usually not printed solid. If strength or stiffness matters, state the required wall count or infill, or ask for a solid part.
- Overhangs and supports: surfaces more than about 45° from vertical need supports, which leave marks. Mark the cosmetic faces so supports go elsewhere.
- Holes and fits: printed holes come out slightly undersize and faceted. Drill or ream fit-critical holes and leave clearance on mating parts, as Uretyco's 3D printing guidance recommends.
- Threads: use heat-set inserts or post-machining for reliable threads; printed threads suit low-load use only.
Tolerances and surface
Without a drawing tolerance, Uretyco applies the FDM default of ±0.5 mm or ±0.5%, whichever is greater; actual results vary with technology, material shrinkage, orientation, part size, supports and post-processing, so fit-critical features should be tested before production. PLA is among the most dimensionally stable FDM materials because it hardly warps. Layer lines remain visible on every FDM part; for smooth visual models, SLA resin is the better process.
Finishing options
PLA does not respond to the acetone vapor smoothing used on ABS and ASA, so smooth surfaces come from mechanical finishing and coatings.
| Finish | What it adds | Notes for PLA |
|---|---|---|
| As-printed | Lowest cost | Visible layer lines and support marks. |
| Sanded | Smoother surface, fainter layer lines | Wet sanding avoids frictional heat, which softens PLA. |
| Primed and painted | Color match, uniform appearance | The usual finish for presentation models; specify a RAL code or sample. |
| Annealed | Higher heat resistance | Raises heat deflection temperature but causes shrinkage and warping; rarely worth it for precise parts. |
A car interior in summer, a sunny window or a spot next to a motor can exceed PLA's glass transition within hours. Parts sag, warp or lose their fit. Use ASA or a powder-bed nylon for parts that get hot, and PETG only where conditions are mildly warm.
Cost and lead-time drivers
PLA is the lowest-cost FDM material, so price is driven almost entirely by the print itself:
- Volume and build time: part size, wall count, infill and layer height set machine time; hollow or lightly filled parts print faster.
- Supports and orientation: support-heavy geometry adds material, print time and clean-up.
- Post-processing: sanding, priming and painting are manual work and often cost more than the print.
- Size and color: small parts in common colors are fast; large parts and special colors take longer.
PLA vs. other prototyping materials
| Material | Heat resistance | Toughness | Outdoor / UV | Printing | Best for |
|---|---|---|---|---|---|
| PLA (FDM) | ≈ 50 °C | Low; brittle | Poor | Easiest; minimal warp | Visual prototypes, fit checks |
| PETG (FDM) | ≈ 60–70 °C | Good | Moderate | Easy | Functional parts, light outdoor use |
| ASA (FDM) | ≈ 85 °C | Good | Excellent | Needs an enclosed printer; can warp | Outdoor housings |
| ABS (FDM) | ≈ 60–80 °C | Good | Poor | Needs an enclosed printer; can warp | Indoor functional parts, smoothed finishes |
| PA12 (MJF/SLS) | ≈ 80–100 °C | Very good | Good | Powder bed; no supports | Durable functional parts |
| Standard resin (SLA) | ≈ 50–60 °C | Low; brittle | Poor | Very smooth, fine detail | Cosmetic models |
When not to choose PLA
Anything that gets warmer than about 50 °C: cars, sunny windows, machinery, dishwashers. Outdoor use beyond a few months. Snap-fits, living hinges and impact-loaded parts: PLA cracks. Sustained loads such as brackets under constant weight or press fits: PLA creeps. Food-contact parts: layer crevices trap bacteria, so FDM parts should not be treated as food-safe.
Typical applications
- Visual and form-study prototypes.
- Fit checks for assemblies that stay at room temperature.
- Architectural, presentation and display models.
- Indoor jigs, gauges, organizers and light-duty fixtures.
- Educational models and packaging mock-ups.
Specifying PLA on Uretyco
- 1Upload STL, 3MF or STEP
Check units and scale; 3MF keeps color and unit data, and STEP helps when accuracy matters.
- 2Select PLA and describe the use
Tell the AI assistant about appearance, loads and temperature; it can point to PETG or ASA if PLA is marginal.
- 3Note orientation, infill and cosmetic faces
Add a drawing or notes for fit-critical dimensions, threads or inserts.
FAQ
Will a PLA part survive in a hot car?
No. A closed car in summer easily exceeds PLA's glass transition, and parts sag or warp within hours. Use ASA or a powder-bed nylon instead.
Is PLA biodegradable?
Only under industrial composting conditions with high temperature and humidity. In soil, water or a home compost bin it persists for a long time, so treat it like other plastics at end of life.
Is PLA food-safe?
The base polymer is made in food-contact grades, but FDM parts have layer crevices that trap bacteria, and colorants and printer components are not controlled for food contact. Do not use FDM PLA parts for repeated food contact.
Can PLA be used for functional parts?
For light, room-temperature duty, yes: jigs, fixtures and brackets that are not impact-loaded. For anything that flexes, gets warm or carries a sustained load, PETG, ASA or a powder-bed nylon will last longer.
What is PLA+ and when should I choose it?
PLA+ is a common name for toughened or modified PLA: manufacturers blend in impact modifiers or other polymers and adjust the additive package so the material is less brittle. Datasheets usually show clearly higher impact strength and elongation at break and better layer adhesion, at slightly lower stiffness and with heat resistance close to standard PLA. There is no standard definition, so properties vary from brand to brand and should be read from the specific datasheet. Choose PLA+ for room-temperature prototypes, fixtures and clips that must survive handling or occasional knocks; for heat, outdoor use or sustained load, PETG, ASA or a powder-bed nylon remain the better choice. If you need a toughened grade, state it in the order notes; the grade is confirmed in the quote.
Related resources
- PETGTougher, more heat-resistant FDM material.
- ASAUV-stable FDM material for outdoor parts.
- PA12 NylonDurable powder-bed parts.
- Standard SLA ResinSmoother visual models.
- 3D PrintingTechnologies, files and cost drivers.
- Choosing the Right ProcessCompare processes by use case.
- Supported File FormatsSTL, 3MF and STEP for printing.
- Material Selection GuideChoose by requirement, not by name.
Related materials